Dimension
Property | Value |
---|---|
Dimensions | Please feel free to check the figure on the right side of the material page for more details. |
Mechanical
Property | Value | Comment |
---|---|---|
Elongation | 17 % Show Supplier Material materials with Elongation of 17 % | min. | for thickness 0.3-0.5 mm | Transverse | A80 |
19 % Show Supplier Material materials with Elongation of 19 % | min. | for thickness 0.5-0.7 mm | Transverse | A80 | |
21 % Show Supplier Material materials with Elongation of 21 % | min. | for thickness 0.7-3 mm | Transverse | A80 | |
Tensile strength | 380 - 480 MPa Show Supplier Material materials with Tensile strength of 380 - 480 MPa | for thickness 0.3-3 mm | Transverse |
Yield strength | 300 - 380 MPa Show Supplier Material materials with Yield strength of 300 - 380 MPa | for thickness 0.3-3 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 0.015 % Show Supplier Material materials with Aluminium of 0.015 % | min. |
Carbon | 0.12 % Show Supplier Material materials with Carbon of 0.12 % | max. |
Manganese | 1.4 % Show Supplier Material materials with Manganese of 1.4 % | max. |
Niobium | 0.09 % Show Supplier Material materials with Niobium of 0.09 % | max. |
Phosphorus | 0.03 % Show Supplier Material materials with Phosphorus of 0.03 % | max. |
Silicon | 0.5 % Show Supplier Material materials with Silicon of 0.5 % | max. |
Sulfur | 0.025 % Show Supplier Material materials with Sulfur of 0.025 % | max. |
Titanium | 0.15 % Show Supplier Material materials with Titanium of 0.15 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | Because Alusi® can resist high temperatures, it is particularly suitable for use in thermal shielding. However, Alusi® also has many other applications: Alusi® can be supplied oiled and/or passivated, or with an Easyfilm® thin organic coating (please see data sheet E80 for the specific properties of Easyfilm®). Under certain conditions, Alusi® is suitable for food contact, as specified in the Regulation (EC) No. 1935/2004 and French standard NF A 36-712-2. Please contact us for further information on this subject. | |
Coating | ||
Other | Recommendations for use Alusi® must be transported and stored in a sheltered, moisture-free environment. The forming and joining techniques currently used for uncoated steel are also suitable for Alusi®. Alusi® coated steel can be welded using various types of resistance welding processes (spot, seam, butt welding). TIG, MIG, MAG, High Frequency Induction welding and laser welding are also suitable. When supplied oiled, Alusi® needs degreasing and surface treatment before painting. Alusi® coated with an Easyfilm® thin organic coating can be painted directly, without any prior surface treatment. However, the paint must be compatible with the Easyfilm® resin. |