EN 10225 Grade S355G7 normalized or normalized formed (+N)

Want to keep this datasheet? Save it now in your required format

Description

This steel is thermomechanically rolled (M) or normalised (N).

Our products are studied to improve workability and weldability.

Related Standards

Equivalent Materials

This material data has been provided by ArcelorMittal.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyValueComment

Carbon equivalent (CEV)

0.43 [-]

Show Supplier Material materials with Carbon equivalent (CEV) of 0.43 [-]

Product

Weld cracking parameter

0.24 [-]

Show Supplier Material materials with Weld cracking parameter of 0.24 [-]

Product

Carbon equivalent note

CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Cu+Ni)/15 and PCM = C + Si/30 + (Cr+Mn+Cu)/20 + Ni/60 + Mo/15 + V/10 + 5B

Mechanical

PropertyTemperatureValueComment

Charpy impact energy

-40 °C

50 J

Show Supplier Material materials with Charpy impact energy of 50 J

min. | for thickness 5-80 mm | Transverse

Elongation

22 %

Show Supplier Material materials with Elongation of 22 %

min. A5.65√So | for thickness 5-80 mm | Transverse

Tensile strength

470 - 630 MPa

Show Supplier Material materials with Tensile strength of 470 - 630 MPa

for thickness 5-80 mm | Transverse

Yield strength

325 MPa

Show Supplier Material materials with Yield strength of 325 MPa

min. | for thickness 63-80 mm | Transverse

335 MPa

Show Supplier Material materials with Yield strength of 335 MPa

min. | for thickness 40-63 mm | Transverse

345 MPa

Show Supplier Material materials with Yield strength of 345 MPa

min. | for thickness 25-40 mm | Transverse

355 MPa

Show Supplier Material materials with Yield strength of 355 MPa

min. | for thickness 5-25 mm | Transverse

Yield to strength ratio

0.85 [-]

Show Supplier Material materials with Yield to strength ratio of 0.85 [-]

max | for thickness 16-25 mm | Transverse

0.87 [-]

Show Supplier Material materials with Yield to strength ratio of 0.87 [-]

max | for thickness 5-16 mm | Transverse

Chemical properties

PropertyValueComment

Aluminium

0.015 - 0.055 %

Show Supplier Material materials with Aluminium of 0.015 - 0.055 %

for thickness 5-80 mm

Carbon

0.14 %

Show Supplier Material materials with Carbon of 0.14 %

max. | for thickness 5-80 mm

Chromium

0.25 %

Show Supplier Material materials with Chromium of 0.25 %

max. | for thickness 5-80 mm

Copper

0.3 %

Show Supplier Material materials with Copper of 0.3 %

max. | for thickness 5-80 mm

Manganese

1 - 1.65 %

Show Supplier Material materials with Manganese of 1 - 1.65 %

for thickness 5-80 mm

Molybdenum

0.08 %

Show Supplier Material materials with Molybdenum of 0.08 %

max. | for thickness 5-80 mm

Nickel

0.5 %

Show Supplier Material materials with Nickel of 0.5 %

max. | for thickness 5-80 mm

Niobium

0.04 %

Show Supplier Material materials with Niobium of 0.04 %

max. | for thickness 5-80 mm

Nitrogen

0.01 %

Show Supplier Material materials with Nitrogen of 0.01 %

max. | for thickness 5-80 mm

Phosphorus

0.02 %

Show Supplier Material materials with Phosphorus of 0.02 %

max. | for thickness 5-80 mm

Silicon

0.15 - 0.55 %

Show Supplier Material materials with Silicon of 0.15 - 0.55 %

for thickness 5-80 mm

Sulfur

0.01 %

Show Supplier Material materials with Sulfur of 0.01 %

max. | for thickness 5-80 mm

Titanium

0.025 %

Show Supplier Material materials with Titanium of 0.025 %

max. | for thickness 5-80 mm

Vanadium

0.06 %

Show Supplier Material materials with Vanadium of 0.06 %

max. | for thickness 5-80 mm

Technological properties

Property
Application areas

Offshore structures such as platforms and equipment for new offshore windmill towers.

Chemical composition

  • A ratio Al/N ≥ 2 shall be applied
  • The sum of the percentages by mass of the four elements chromium, nickel, copper and molybdenum shall not exceed 0.90%.
  • The sum of the percentages by mass of the two elements niobium and vanadium shall not exceed 0.06% and the sum of the percentages by mass of the three elements niobium, titanium and vanadium shall not exceed 0.08%.

    The above chemical properties are based on cast analysis data. Product analysis may be requested at the time of order.

  • Delivery condtion

    For the dimensions available please visit Dimension tables (see Table A). Table A with a thickness range as indicated in the Mechanical properties.

    Other

    Available options

    Options available (after previous agreement):

  • Ultrasonic testing
  • Reduced carbon equivalent (CEV) or parameter crack measurement (PCM) value
  • Transversal impact test
  • Improved deformation properties perpendicular to the surface of the product as per EN 10164 (Z test)
  • Post-weld heat treatment test (PWHT)
  • Other options specified in the standard