General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 8.47 g/cm³ Show Material materials with Density of 8.47 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 23.0 °C | 100 GPa Show Material materials with Elastic modulus of 100 GPa |
Elongation | 23.0 °C | 20 % Show Material materials with Elongation of 20 % |
Hardness, Vickers | 23.0 °C | 130 [-] Show Material materials with Hardness, Vickers of 130 [-] |
Tensile strength | 23.0 °C | 520 MPa Show Material materials with Tensile strength of 520 MPa |
Yield strength Rp0.2 | 23.0 °C | 230 MPa Show Material materials with Yield strength Rp0.2 of 230 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Melting point | 940 - 980 °C Show Material materials with Melting point of 940 - 980 °C | |
Thermal conductivity | 23.0 °C | 46 W/(m·K) Show Material materials with Thermal conductivity of 46 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 23.0 °C | 5.22E+6 S/m Show Material materials with Electrical conductivity of 5.22E+6 S/m |
Electrical resistivity | 23.0 °C | 1.8E-7 Ω·m Show Material materials with Electrical resistivity of 1.8E-7 Ω·m |
Specific Electrical conductivity | 9 % IACS Show Material materials with Specific Electrical conductivity of 9 % IACS |
Magnetic
Property | Temperature | Value | Comment |
---|---|---|---|
Relative magnetic permeability | 23.0 °C | 1.05 [-] Show Material materials with Relative magnetic permeability of 1.05 [-] | max. |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Copper | 44 - 47 % Show Material materials with Copper of 44 - 47 % | ||
Iron | 0.4 % Show Material materials with Iron of 0.4 % | max. | |
Lead | 1 - 2.5 % Show Material materials with Lead of 1 - 2.5 % | ||
Manganese | 0.2 - 0.5 % Show Material materials with Manganese of 0.2 - 0.5 % | ||
Nickel | 9 - 11 % Show Material materials with Nickel of 9 - 11 % | ||
Zinc | Balance |
Technological properties
Property | ||
---|---|---|
Application areas | Frequently used applications of NS101 include gears, pinions, clock and watch parts, screws and other types of fasteners, hot stampings and forgings, keys, lock parts, door furniture, grills, decorative and architectural metalwork, darts, fishing tackle, camera, binocular and microscope parts, musical instrument valves and fittings, electrical and electronic pins and connectors and switchgear components. | |
Corrosion properties | Good corrosion resistance | |
General machinability | Very good machining and hot stamping characteristics |