Mechanical
Property | Value | Comment |
---|---|---|
Hardness, Brinell | 280 - 325 [-] Show Supplier Material materials with Hardness, Brinell of 280 - 325 [-] | delivery condition |
Tensile strength | 890 - 1030 MPa Show Supplier Material materials with Tensile strength of 890 - 1030 MPa | according to EN ISO 18265 table B2 |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 1.19e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.19e-05 1/K | 20-100 °C | |
1.25e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.25e-05 1/K | 20-200 °C | ||
1.31e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.31e-05 1/K | 20-300 °C | ||
1.36e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | 20-400 °C | ||
1.41e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | 20-500 °C | ||
1.41e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | 20-600 °C | ||
Specific heat capacity | 460 J/(kg·K) Show Supplier Material materials with Specific heat capacity of 460 J/(kg·K) | ||
Thermal conductivity | 20 °C | 34 W/(m·K) Show Supplier Material materials with Thermal conductivity of 34 W/(m·K) | |
100 °C | 32 W/(m·K) Show Supplier Material materials with Thermal conductivity of 32 W/(m·K) | ||
200 °C | 33 W/(m·K) Show Supplier Material materials with Thermal conductivity of 33 W/(m·K) | ||
300 °C | 34 W/(m·K) Show Supplier Material materials with Thermal conductivity of 34 W/(m·K) | ||
400 °C | 34 W/(m·K) Show Supplier Material materials with Thermal conductivity of 34 W/(m·K) |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Carbon | 0.35 - 0.45 % Show Supplier Material materials with Carbon of 0.35 - 0.45 % | limiting values | |
0.4 % Show Supplier Material materials with Carbon of 0.4 % | auxiliary data for 100 mm plate thickness | ||
Chromium | 1.8 - 2.1 % Show Supplier Material materials with Chromium of 1.8 - 2.1 % | limiting values | |
1.9 % Show Supplier Material materials with Chromium of 1.9 % | auxiliary data for 100 mm plate thickness | ||
Iron | Balance | ||
Manganese | 1.3 - 1.6 % Show Supplier Material materials with Manganese of 1.3 - 1.6 % | limiting values | |
1.55 % Show Supplier Material materials with Manganese of 1.55 % | auxiliary data for 100 mm plate thickness | ||
Molybdenum | 0.15 - 0.25 % Show Supplier Material materials with Molybdenum of 0.15 - 0.25 % | limiting values | |
0.2 % Show Supplier Material materials with Molybdenum of 0.2 % | auxiliary data for 100 mm plate thickness | ||
Nickel | 0.9 - 1.1 % Show Supplier Material materials with Nickel of 0.9 - 1.1 % | limiting values | |
0.95 % Show Supplier Material materials with Nickel of 0.95 % | auxiliary data for 100 mm plate thickness | ||
Phosphorus | 0.015 % Show Supplier Material materials with Phosphorus of 0.015 % | auxiliary data for 100 mm plate thickness | |
0.025 % Show Supplier Material materials with Phosphorus of 0.025 % | max. limiting values | ||
Silicon | 0.2 - 0.4 % Show Supplier Material materials with Silicon of 0.2 - 0.4 % | limiting values | |
0.3 % Show Supplier Material materials with Silicon of 0.3 % | auxiliary data for 100 mm plate thickness | ||
Sulfur | 0.001 % Show Supplier Material materials with Sulfur of 0.001 % | auxiliary data for 100 mm plate thickness | |
0.002 % Show Supplier Material materials with Sulfur of 0.002 % | max. limiting values | ||
Vanadium | 0.05 % Show Supplier Material materials with Vanadium of 0.05 % | auxiliary data for 100 mm plate thickness (alloyed depending on dimensions) |
Technological properties
Property | ||
---|---|---|
Application areas | For the construction of plastic molds with superior surface requirements on molds. | |
Chemical composition | Vanadium alloyed depending on dimension. | |
Delivery condtion | DIMO 2738 is supplied in the prehardened (air hardened + tempered) condition. | |
General note | If special requirements, which are not listed in this specification, are to be met by the steel due to its intended use or processing, these requirements are to be agreed before placing the order. The information in this specification is a product description. This specification is updated if necessary. The latest version is available from the mill or as download at www.dillinger.de. | |
Heat Treatment | DIMO 2738 is delivered in the hardened condition; therefore further heat treatment is generally not necessary. This avoids the risks and costs involved by the hardening and tempering of a mold after processing. Should a heat treatment become necessary, recommended data can be found in material data sheet at www.dillinger.de. | |
Other | DIMO 2738 is available as plate with sheared or flame cut edges in the following dimensions: Widths < 1250 mm (49 in) have to be ordered with an even number of plates, Other dimensions available upon request. Unless otherwise agreed, the results are documented in an inspection certificate 3.1 in accordance with EN 10204. Unless otherwise agreed the marking is carried out via steel stamps with at least the following information: | |
Processing history | The DIMO 2738 production route is designed to achieve the excellent properties of this mold steel type with superior surface requirements. DIMO 2738 is characterized by high dimensional stability. The DIMO 2738 production route provides excellent polishability, photoetchability and spark erosion properties. Therefore DIMO 2738 is particularly suitable for molds with superior surface requirements if suitable manufacturing processes are employed. The good sulfidic and oxidic cleanliness and the modification of the few remaining inclusions by the calcium treatment lead to good machinability and minimize the tool wear. Thicknesses ≥ 100 mm show a better through-hardening compared to DIMO 2311. These properties can only be achieved by the combination of the following DIMO 2738-production steps: | |
Surface condition | Surface quality: Unless otherwise agreed, the specifications will be in accordance with EN 10163-2 class A, subclass 3. Shot blasting of upper and lower surface of the plate and shop priming are possible on request. | |
Testings | Unless otherwise agreed, the results are documented in an inspection certificate 3.1 in accordance with EN 10204. | |
Tolerances | Unless otherwise agreed, tolerances are in accordance with EN 10029 / ASTM A 6 with the following restrictions: |