Super Invar 32-5 is a low expansion alloy consisting of 32% nickel, 5% cobalt, and balance iron. Super Invar Alloy exhibits minimum thermal expansion at room temperatures (one half of Invar Alloy), as well as thermal expansion properties less than that of Invar Alloy in the 67/203°F (-55/95°C) temperature range.

Related Standards

Equivalent Materials

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.15 g/cm³

Show Material materials with Density of 8.15 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

145 GPa

Show Material materials with Elastic modulus of 145 GPa

Elongation

23.0 °C

40 %

Show Material materials with Elongation of 40 %

in 2 in.

Hardness, Rockwell B

23.0 °C

75 [-]

Show Material materials with Hardness, Rockwell B of 75 [-]

Tensile strength

23.0 °C

483 MPa

Show Material materials with Tensile strength of 483 MPa

Yield strength

23.0 °C

276 MPa

Show Material materials with Yield strength of 276 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

8.4E-7 1/K

Show Material materials with Coefficient of thermal expansion of 8.4E-7 1/K

from 20°C to the mentioned temperature

150.0 °C

1.17E-6 1/K

Show Material materials with Coefficient of thermal expansion of 1.17E-6 1/K

from 20°C to the mentioned temperature

200.0 °C

1.72E-6 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-6 1/K

from 20°C to the mentioned temperature

250.0 °C

2.53E-6 1/K

Show Material materials with Coefficient of thermal expansion of 2.53E-6 1/K

from 20°C to the mentioned temperature

300.0 °C

4.16E-6 1/K

Show Material materials with Coefficient of thermal expansion of 4.16E-6 1/K

from 20°C to the mentioned temperature

350.0 °C

5.74E-6 1/K

Show Material materials with Coefficient of thermal expansion of 5.74E-6 1/K

from 20°C to the mentioned temperature

400.0 °C

7.03E-6 1/K

Show Material materials with Coefficient of thermal expansion of 7.03E-6 1/K

from 20°C to the mentioned temperature

500.0 °C

8.99E-6 1/K

Show Material materials with Coefficient of thermal expansion of 8.99E-6 1/K

from 20°C to the mentioned temperature

550.0 °C

1.06E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.06E-5 1/K

from 20°C to the mentioned temperature

700.0 °C

1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K

from 20°C to the mentioned temperature

800.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

from 20°C to the mentioned temperature

900.0 °C

1.3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K

from 20°C to the mentioned temperature

Melting point

1427 °C

Show Material materials with Melting point of 1427 °C

Specific heat capacity

23.0 °C

502 J/(kg·K)

Show Material materials with Specific heat capacity of 502 J/(kg·K)

Thermal conductivity

23.0 °C

10 W/(m·K)

Show Material materials with Thermal conductivity of 10 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

8.2E-7 Ω·m

Show Material materials with Electrical resistivity of 8.2E-7 Ω·m

Magnetic

PropertyValue

Curie temperature

245 °C

Show Material materials with Curie temperature of 245 °C

Chemical properties

PropertyValue

Carbon

0.05 %

Show Material materials with Carbon of 0.05 %

Chromium

0.25 %

Show Material materials with Chromium of 0.25 %

Cobalt

5 %

Show Material materials with Cobalt of 5 %

Iron

Balance

Nickel

32 %

Show Material materials with Nickel of 32 %

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Technological properties

Property
Application areas

Common applications of Super Invar 32-5 are: Optical instruments . Telescopes . Laser instruments and equipment . Ring laser gyroscopes . Laser benches . Positioning devices . Metrology devices . Structural components . Substrates in instrument systems requiring precision measurements