General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 8.3 g/cm³ Show Material materials with Density of 8.3 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 159 GPa Show Material materials with Elastic modulus of 159 GPa | |
Elongation | 23.0 °C | 35 % Show Material materials with Elongation of 35 % | in 2 in. |
Hardness, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Hardness, Rockwell B of 80 [-] | |
Tensile strength | 23.0 °C | 552 MPa Show Material materials with Tensile strength of 552 MPa | |
Yield strength | 23.0 °C | 276 MPa Show Material materials with Yield strength of 276 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | from 30°C to the mentioned temperature |
150.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 1.04E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 1.04E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 1.01E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 1.07E-5 - 9.6E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.07E-5 - 9.6E-5 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 1.01E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.01E-5 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1E-5 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 1.04E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 1.02E-5 - 1.07E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 - 1.07E-5 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.17E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.17E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.33E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.33E-5 1/K | from 30°C to the mentioned temperature | |
1009.0 °C | 1.42E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.42E-5 1/K | from 30°C to the mentioned temperature | |
Melting point | 1427 °C Show Material materials with Melting point of 1427 °C | ||
Specific heat capacity | 23.0 °C | 502 J/(kg·K) Show Material materials with Specific heat capacity of 502 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 14 W/(m·K) Show Material materials with Thermal conductivity of 14 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 23.0 °C | 4.4E-7 Ω·m Show Material materials with Electrical resistivity of 4.4E-7 Ω·m |
Magnetic
Property | Value |
---|---|
Curie temperature | 530 °C Show Material materials with Curie temperature of 530 °C |
Chemical properties
Property | Value |
---|---|
Carbon | 0.05 % Show Material materials with Carbon of 0.05 % |
Chromium | 0.03 % Show Material materials with Chromium of 0.03 % |
Iron | Balance |
Nickel | 50.5 % Show Material materials with Nickel of 50.5 % |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 52: Pin feed-throughs for semiconductor devices, glass-to-metal sealing with soft glass for mercury switches and semiconductor devices |