General
Property | Value | Related Standards | Shape |
---|---|---|---|
Density | 4.428999999999999 g/cm³ Show Material materials with Density of 4.428999999999999 g/cm³ | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
4.43 g/cm³ Show Material materials with Density of 4.43 g/cm³ | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
Dimension
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Diameter | 5 mm Show Material materials with Diameter of 5 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Tube | ||
7 mm Show Material materials with Diameter of 7 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar | |||
25.4 mm Show Material materials with Diameter of 25.4 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
115 mm Show Material materials with Diameter of 115 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar | |||
125 mm Show Material materials with Diameter of 125 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
130 mm Show Material materials with Diameter of 130 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet, Tube | |||
350 mm Show Material materials with Diameter of 350 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
Dimensions | 15-65 mm diameter up to 6000 mm length °C | 7-14.5 mm diameter up to 3000 mm length | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar | |
Length | 1000 mm Show Material materials with Length of 1000 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Tube | ||
1500 mm Show Material materials with Length of 1500 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate | |||
3000 mm Show Material materials with Length of 3000 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
4500 mm Show Material materials with Length of 4500 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
5000 mm Show Material materials with Length of 5000 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Tube | |||
6000 mm Show Material materials with Length of 6000 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar | max | ||
6500 mm Show Material materials with Length of 6500 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Plate | |||
Wall thickness | 0.5 - 9.0 mm Show Material materials with Wall thickness of 0.5 - 9.0 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Tube | ||
2.5 - 21.0 mm Show Material materials with Wall thickness of 2.5 - 21.0 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Billet | |||
Width | 400 mm Show Material materials with Width of 400 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet | ||
600 mm Show Material materials with Width of 600 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Plate | |||
1524 mm Show Material materials with Width of 1524 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet | |||
1600 mm Show Material materials with Width of 1600 mm | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Plate |
valueMetaData
Property | Value |
---|
Mechanical
Property | Value | Related Standards | Shape |
---|---|---|---|
Elastic modulus | 110.0 - 119.0 GPa Show Material materials with Elastic modulus of 110.0 - 119.0 GPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
114.0 GPa Show Material materials with Elastic modulus of 114.0 GPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate | |
Elongation | 14.0 % Show Material materials with Elongation of 14.0 % | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Hardness, Brinell | 310.0 Show Material materials with Hardness, Brinell of 310.0 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
334.0 Show Material materials with Hardness, Brinell of 334.0 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate | |
Hardness, Rockwell C | 36.0 Show Material materials with Hardness, Rockwell C of 36.0 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Hardness, Vickers | 349.0 Show Material materials with Hardness, Vickers of 349.0 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Poisson's ratio | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Shear modulus | 40.0 GPa Show Material materials with Shear modulus of 40.0 GPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Tensile strength | 862.0 - 1200.0 MPa Show Material materials with Tensile strength of 862.0 - 1200.0 MPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
895.0 MPa Show Material materials with Tensile strength of 895.0 MPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate | |
Yield strength | 830.0 MPa Show Material materials with Yield strength of 830.0 MPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
880.0 MPa Show Material materials with Yield strength of 880.0 MPa | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
Thermal
Property | Value | Related Standards | Shape | Comment |
---|---|---|---|---|
Coefficient of thermal expansion | 7.699999999999999e-06 - 1e-05 1/K Show Material materials with Coefficient of thermal expansion of 7.699999999999999e-06 - 1e-05 1/K | Typical for Titanium Alpha Beta Alloy | ||
Melting point | 1500.0 - 1750.0 °C Show Material materials with Melting point of 1500.0 - 1750.0 °C | Typical for Titanium Alpha Beta Alloy | ||
Specific heat capacity | 560 J/(kg·K) Show Material materials with Specific heat capacity of 560 J/(kg·K) | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate | |
Thermal conductivity | 7.1 W/(m·K) Show Material materials with Thermal conductivity of 7.1 W/(m·K) | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
Chemical properties
Property | Value | Related Standards | Shape |
---|---|---|---|
Aluminium | 5.5 - 6.75 % Show Material materials with Aluminium of 5.5 - 6.75 % | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
6.0 % Show Material materials with Aluminium of 6.0 % | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate | |
Carbon | 0.08 Show Material materials with Carbon of 0.08 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
Hydrogen | 0.0125 Show Material materials with Hydrogen of 0.0125 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
Iron | 0.25 Show Material materials with Iron of 0.25 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate |
0.3 Show Material materials with Iron of 0.3 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate | |
Nitrogen | 0.05 Show Material materials with Nitrogen of 0.05 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
Oxygen | 0.2 Show Material materials with Oxygen of 0.2 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate, Bar, Billet, Tube |
Vanadium | 3.5 - 4.5 % Show Material materials with Vanadium of 3.5 - 4.5 % | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |
4.0 % Show Material materials with Vanadium of 4.0 % | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Bar, Billet, Tube, Sheet, Plate | |
Yttrium | 0.005 Show Material materials with Yttrium of 0.005 | ASME SB-265, AMS 4911, ASME SB-348, AMS 4928, AMS 4965, AMS 4967 | Sheet, Plate |