Titanium UNS R56260 is an Alpha-Beta Alloy and it’s generally regarded as the workhorse alloy of the titanium industry. The alloy is fully heat-treatable in section sizes up to one inch and is used up to approximately 400°C (750°F). Since it is one of the most commonly used alloys (over 70% of all alloy grades melted are a sub-grade of Ti-6-4,) its uses span many aerospace engine and airframe components. Titanium UNS R56260 is also used in lots of non-aerospace applications such as marine, offshore and power generation industries. This Alpha-Beta Alloy combines good corrosion resistance and strength with weldability and fabricability. The alloy is generally available in bar form and it’s typically used in deep sour well applications. This alloy can be hot or cold formed.

Related Standards

This material data has been provided by VSMPO,Matmatch,RMI Titanium Co.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueShapeRelated Standards

Density

4.65 g/cm³

Show Material materials with Density of 4.65 g/cm³

Bar, Billet

4.65 g/cm³

Show Material materials with Density of 4.65 g/cm³

AMS 4981B, MIL-T 9047G

Dimension

PropertyTemperatureValueShapeComment

Diameter

7 mm

Show Material materials with Diameter of 7 mm

Bar

115 mm

Show Material materials with Diameter of 115 mm

Bar

130 mm

Show Material materials with Diameter of 130 mm

Billet

350 mm

Show Material materials with Diameter of 350 mm

Billet

Dimensions

15-65 mm diameter up to 6000 mm length °C

7-14.5 mm diameter up to 3000 mm length

Bar

Length

3000 mm

Show Material materials with Length of 3000 mm

Billet

4500 mm

Show Material materials with Length of 4500 mm

Billet

6000 mm

Show Material materials with Length of 6000 mm

Bar

max

Mechanical

PropertyValueShapeRelated Standards

Elastic modulus

114.0 GPa

Show Material materials with Elastic modulus of 114.0 GPa

Bar, Billet

114 GPa

Show Material materials with Elastic modulus of 114 GPa

AMS 4981B, MIL-T 9047G

Elongation

13.0 %

Show Material materials with Elongation of 13.0 %

Bar, Billet

Hardness, Brinell

360.0

Show Material materials with Hardness, Brinell of 360.0

Bar, Billet

Hardness, Rockwell C

39.0 [-]

Show Material materials with Hardness, Rockwell C of 39.0 [-]

Bar, Billet

Hardness, Vickers

376.0

Show Material materials with Hardness, Vickers of 376.0

Bar, Billet

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Bar, Billet

Shear modulus

42.9 GPa

Show Material materials with Shear modulus of 42.9 GPa

Bar, Billet

Tensile strength

1172.0 MPa

Show Material materials with Tensile strength of 1172.0 MPa

AMS 4981B, MIL-T 9047G

1210.0 MPa

Show Material materials with Tensile strength of 1210.0 MPa

Bar, Billet

Yield strength

1103.0 MPa

Show Material materials with Yield strength of 1103.0 MPa

AMS 4981B, MIL-T 9047G

1120.0 MPa

Show Material materials with Yield strength of 1120.0 MPa

Bar, Billet

Thermal

PropertyTemperatureValueRelated StandardsShape

Coefficient of thermal expansion

20 °C

0.0000094 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000094 1/K

AMS 4981B, MIL-T 9047G

20 °C

0.0000103 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000103 1/K

AMS 4981B, MIL-T 9047G

20 °C

0.0000104 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000104 1/K

AMS 4981B, MIL-T 9047G

100 °C

0.0000094 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000094 1/K

AMS 4981B, MIL-T 9047G

315 °C

0.0000103 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000103 1/K

AMS 4981B, MIL-T 9047G

538 °C

0.0000104 1/K

Show Material materials with Coefficient of thermal expansion of 0.0000104 1/K

AMS 4981B, MIL-T 9047G

Melting point

1593.0 °C

Show Material materials with Melting point of 1593.0 °C

AMS 4981B, MIL-T 9047G

1595.0 - 1675.0 °C

Show Material materials with Melting point of 1595.0 - 1675.0 °C

Bar, Billet

Specific heat capacity

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

AMS 4981B, MIL-T 9047G

Thermal conductivity

7.7 W/(m·K)

Show Material materials with Thermal conductivity of 7.7 W/(m·K)

AMS 4981B, MIL-T 9047G

Bar, Billet

Electrical

PropertyValueRelated Standards

Electrical resistivity

2e-06 Ω·m

Show Material materials with Electrical resistivity of 2e-06 Ω·m

AMS 4981B, MIL-T 9047G

Chemical properties

PropertyValueRelated StandardsShape

Aluminium

5.5 - 6.5 %

Show Material materials with Aluminium of 5.5 - 6.5 %

AMS 4981B, MIL-T 9047G

6.0 %

Show Material materials with Aluminium of 6.0 %

Bar, Billet

Carbon

0.04

Show Material materials with Carbon of 0.04

AMS 4981B, MIL-T 9047G

Hydrogen

0.0125

Show Material materials with Hydrogen of 0.0125

AMS 4981B, MIL-T 9047G

Iron

0.15

Show Material materials with Iron of 0.15

AMS 4981B, MIL-T 9047G

Molybdenum

5.5 - 6.5 %

Show Material materials with Molybdenum of 5.5 - 6.5 %

AMS 4981B, MIL-T 9047G

6.0 %

Show Material materials with Molybdenum of 6.0 %

Bar, Billet

Nitrogen

0.04

Show Material materials with Nitrogen of 0.04

AMS 4981B, MIL-T 9047G

Oxygen

0.5

Show Material materials with Oxygen of 0.5

AMS 4981B, MIL-T 9047G

Tin

1.75 - 2.25 %

Show Material materials with Tin of 1.75 - 2.25 %

AMS 4981B, MIL-T 9047G

2.0 %

Show Material materials with Tin of 2.0 %

Bar, Billet

Zirconium

3.5 - 4.5 %

Show Material materials with Zirconium of 3.5 - 4.5 %

AMS 4981B, MIL-T 9047G

4.0 %

Show Material materials with Zirconium of 4.0 %

Bar, Billet