DIN 17740 Grade LC-Ni99.6 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The material LC-Ni99.6 with the material number 2.406 is applied in the form of strips, sheets, tubes, bars, wires and forgings for corrosion-resistant construction components, built-in parts for light bulbs and thermionic valves. It is similar to the material LC-Ni99, yet with a minor change in the chemical composition in order to increase the purity. In comparison to Ni99.2 or Ni99.6, the carbon content is lower and prevents embrittlement by intergranular carbon at temperatures of more than 315 °C and reduces the hardness, too, so that LC-Ni99.6 is especially suitable for cold-formed parts. Typical fields of application are sodium hydroxyde production (evaporators), the chlorine production (membrane cell cathodes) as well as the production of vinyl-chloride monomers (VCM), hydrogen chloride, soap and washing agents. Wide application in the food processing, too. Processing properties: Formability: very good Weldability: good

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.9 g/cm³

Show Material materials with Density of 8.9 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

208 GPa

Show Material materials with Elastic modulus of 208 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation A100

20.0 °C

20 - 30 %

Show Material materials with Elongation A100 of 20 - 30 %

Hardness, Brinell

20.0 °C

130 [-]

Show Material materials with Hardness, Brinell of 130 [-]

Tensile strength

20.0 °C

340 - 400 MPa

Show Material materials with Tensile strength of 340 - 400 MPa

Yield strength Rp0.2

20.0 °C

80 MPa

Show Material materials with Yield strength Rp0.2 of 80 MPa

100.0 °C

70 MPa

Show Material materials with Yield strength Rp0.2 of 70 MPa

200.0 °C

65 MPa

Show Material materials with Yield strength Rp0.2 of 65 MPa

300.0 °C

60 MPa

Show Material materials with Yield strength Rp0.2 of 60 MPa

400.0 °C

55 MPa

Show Material materials with Yield strength Rp0.2 of 55 MPa

Yield strength Rp1.0

20.0 °C

105 MPa

Show Material materials with Yield strength Rp1.0 of 105 MPa

100.0 °C

95 MPa

Show Material materials with Yield strength Rp1.0 of 95 MPa

200.0 °C

90 MPa

Show Material materials with Yield strength Rp1.0 of 90 MPa

300.0 °C

85 MPa

Show Material materials with Yield strength Rp1.0 of 85 MPa

400.0 °C

80 MPa

Show Material materials with Yield strength Rp1.0 of 80 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

8.5E-6 - 1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 8.5E-6 - 1.4E-5 1/K

Typical for Pure/Low Nickel Alloy

Melting point

1400 - 1500 °C

Show Material materials with Melting point of 1400 - 1500 °C

Typical for Pure/Low Nickel Alloy

Specific heat capacity

20.0 °C

456 J/(kg·K)

Show Material materials with Specific heat capacity of 456 J/(kg·K)

Thermal conductivity

20.0 °C

79 W/(m·K)

Show Material materials with Thermal conductivity of 79 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

9.5E-8 Ω·m

Show Material materials with Electrical resistivity of 9.5E-8 Ω·m

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Cobalt

1 %

Show Material materials with Cobalt of 1 %

Copper

0.15 %

Show Material materials with Copper of 0.15 %

Iron

0.25 %

Show Material materials with Iron of 0.25 %

Magnesium

0.15 %

Show Material materials with Magnesium of 0.15 %

Manganese

0.35 %

Show Material materials with Manganese of 0.35 %

Nickel

98.6 %

Show Material materials with Nickel of 98.6 %

Silicon

0.15 %

Show Material materials with Silicon of 0.15 %

Sulfur

5E-3 %

Show Material materials with Sulfur of 5E-3 %

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %