DIN 17744 Grade NiCr20CuMo stabilized

Want to keep this datasheet? Save it now in your required format

Description

The material NiCr20CuMo with the material number 2.4660 is applied in the form of strips, sheets, tubes, bars, wires and forgings for corrosion-resistant construction components. The alloy has an excellent resistance to corrosion in sulphuric, phosphoric and organic acids as well as in aqueous solutions of their salts. The resistance to nitric acid is good as well. As a result of the tailored chemical composition, the alloy also shows excellent resistance to intercrystalline corrosion and stress cracking corrosion. The molybdenum content ensures good resistance to pitting and crevice corrosion. NiCr20CuMo is applied in a wide range at temperatures of up to about 500 °C. Typical fields of application are e.g. plants for the production of sulphuric acid as well as processes that are based on sulphuric acid, such as, among others, extraction columns in the amino acid production and for the production of drugs, plants for the production of synthetic man-made materials and for the production of food as well as heat exchangers in refineries and for the production of phosphoric and hydrofluoric acid. Processing properties: Formability: good Weldability: satisfactory

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.1 g/cm³

Show Material materials with Density of 8.1 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Elongation

20.0 °C

30 %

Show Material materials with Elongation of 30 %

100.0 °C

40 %

Show Material materials with Elongation of 40 %

200.0 °C

40 %

Show Material materials with Elongation of 40 %

300.0 °C

40 %

Show Material materials with Elongation of 40 %

Hardness, Brinell

20.0 °C

217 [-]

Show Material materials with Hardness, Brinell of 217 [-]

Reduction of area

20.0 °C

50 %

Show Material materials with Reduction of area of 50 %

Tensile strength

20.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

100.0 °C

520 MPa

Show Material materials with Tensile strength of 520 MPa

200.0 °C

500 MPa

Show Material materials with Tensile strength of 500 MPa

300.0 °C

480 MPa

Show Material materials with Tensile strength of 480 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

200.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

300.0 °C

140 MPa

Show Material materials with Yield strength Rp0.2 of 140 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.5E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.5E-5 1/K

200.0 °C

1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 1/K

300.0 °C

1.63E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.63E-5 1/K

400.0 °C

1.68E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K

500.0 °C

1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K

600.0 °C

1.74E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.74E-5 1/K

700.0 °C

1.76E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.76E-5 1/K

800.0 °C

1.78E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.78E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 500 °C

Show Material materials with Max service temperature, long of 0 - 500 °C

Melting point

1200 - 1480 °C

Show Material materials with Melting point of 1200 - 1480 °C

Typical for Nickel Chromium Iron Alloy

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

12.3 W/(m·K)

Show Material materials with Thermal conductivity of 12.3 W/(m·K)

100.0 °C

13.1 W/(m·K)

Show Material materials with Thermal conductivity of 13.1 W/(m·K)

200.0 °C

14.8 W/(m·K)

Show Material materials with Thermal conductivity of 14.8 W/(m·K)

300.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

400.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

500.0 °C

19.7 W/(m·K)

Show Material materials with Thermal conductivity of 19.7 W/(m·K)

600.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

Chemical properties

PropertyValue

Carbon

0.07 %

Show Material materials with Carbon of 0.07 %

Chromium

19 - 21 %

Show Material materials with Chromium of 19 - 21 %

Cobalt

1.5 %

Show Material materials with Cobalt of 1.5 %

Copper

3 - 4 %

Show Material materials with Copper of 3 - 4 %

Iron

28.4 %

Show Material materials with Iron of 28.4 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 3 %

Show Material materials with Molybdenum of 2 - 3 %

Nickel

32 - 38 %

Show Material materials with Nickel of 32 - 38 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %