General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 4.505 g/cm³ Show Material materials with Density of 4.505 g/cm³ | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 108.0 - 110.0 GPa Show Material materials with Elastic modulus of 108.0 - 110.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | |
20.0 °C | 108.0 GPa Show Material materials with Elastic modulus of 108.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
200.0 °C | 96.0 - 97.0 GPa Show Material materials with Elastic modulus of 96.0 - 97.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | ||
200.0 °C | 96.0 GPa Show Material materials with Elastic modulus of 96.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
400.0 °C | 82.0 GPa Show Material materials with Elastic modulus of 82.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Elongation | 20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | Annealed | DIN 17851, DIN 17864, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Welded Tube | ||
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Hardness, Brinell | 20.0 °C | 170.0 Show Material materials with Hardness, Brinell of 170.0 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
Reduction of area | 20.0 °C | 30.0 % Show Material materials with Reduction of area of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 30.0 % Show Material materials with Reduction of area of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Shear modulus | 20.0 °C | 45.0 GPa Show Material materials with Shear modulus of 45.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
Tensile strength | 20.0 °C | 460.0 - 590.0 MPa Show Material materials with Tensile strength of 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube | |
20.0 °C | 460.0 - 590.0 MPa Show Material materials with Tensile strength of 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse | |
20.0 °C | 560.0 MPa Show Material materials with Tensile strength of 560.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 460.0 MPa Show Material materials with Tensile strength of 460.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 340.0 MPa Show Material materials with Tensile strength of 340.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 200.0 °C | 9.1e-06 1/K Show Material materials with Coefficient of thermal expansion of 9.1e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
400.0 °C | 9.2e-06 1/K Show Material materials with Coefficient of thermal expansion of 9.2e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
Melting point | 1540.0 - 1715.0 °C Show Material materials with Melting point of 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy | ||||
Specific heat capacity | 20.0 °C | 520.0 J/(kg·K) Show Material materials with Specific heat capacity of 520.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Specific heat capacity of 570.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Specific heat capacity of 630.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Thermal conductivity | 20.0 °C | 22.6 W/(m·K) Show Material materials with Thermal conductivity of 22.6 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 20.9 W/(m·K) Show Material materials with Thermal conductivity of 20.9 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 19.3 W/(m·K) Show Material materials with Thermal conductivity of 19.3 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | 20.0 °C | 5.2e-07 Ω·m Show Material materials with Electrical resistivity of 5.2e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
200.0 °C | 8.7e-07 Ω·m Show Material materials with Electrical resistivity of 8.7e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
400.0 °C | 1.2e-06 Ω·m Show Material materials with Electrical resistivity of 1.2e-06 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.06 Show Material materials with Carbon of 0.06 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Hydrogen | 0.013 Show Material materials with Hydrogen of 0.013 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Iron | 0.25 Show Material materials with Iron of 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Nitrogen | 0.05 Show Material materials with Nitrogen of 0.05 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Oxygen | 0.25 Show Material materials with Oxygen of 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Palladium | 0.15 - 0.25 % Show Material materials with Palladium of 0.15 - 0.25 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Titanium | 98.7 % Show Material materials with Titanium of 98.7 % | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tube, Forging, Rod, Welded Tube |