EN 1179 Grade Zn99.995 F12

Want to keep this datasheet? Save it now in your required format

Description

The fine zinc material Zn99,995, material number 2.2045, is used for fine zinc cast alloys according to DIN 1743, for soluble anodes, for corroding plates, deep-drawing brass, deep-drawing german silver, for zinc sheets and strips and wires as well as for the wire galvanization. Further the material forms the basis for the alloy D-Zn, material number 2.2203, which finds for building purpose use.

Related Standards

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.14 g/cm³

Show Material materials with Density of 7.14 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

105 GPa

Show Material materials with Elastic modulus of 105 GPa

Typical for Zinc

Elongation A10

20.0 °C

50 %

Show Material materials with Elongation A10 of 50 %

Hardness, Brinell

20.0 °C

30 [-]

Show Material materials with Hardness, Brinell of 30 [-]

Poisson's ratio

23.0 °C

0.25 [-]

Show Material materials with Poisson's ratio of 0.25 [-]

Typical for Zinc

Shear modulus

23.0 °C

42 GPa

Show Material materials with Shear modulus of 42 GPa

Typical for Zinc

Tensile strength

20.0 °C

120 MPa

Show Material materials with Tensile strength of 120 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.2E-5 - 2.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.8E-5 1/K

Typical for Zinc

Melting point

380 - 420 °C

Show Material materials with Melting point of 380 - 420 °C

Typical for Zinc

Specific heat capacity

20.0 °C

380 J/(kg·K)

Show Material materials with Specific heat capacity of 380 J/(kg·K)

Thermal conductivity

20.0 °C

113 W/(m·K)

Show Material materials with Thermal conductivity of 113 W/(m·K)

Chemical properties

PropertyValue

Cadmium

3E-3 %

Show Material materials with Cadmium of 3E-3 %

Copper

1E-3 %

Show Material materials with Copper of 1E-3 %

Iron

2E-3 %

Show Material materials with Iron of 2E-3 %

Lead

3E-3 %

Show Material materials with Lead of 3E-3 %

Tin

1E-3 %

Show Material materials with Tin of 1E-3 %

Zinc

100 %