General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 8.2 g/cm³ Show Material materials with Density of 8.2 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 200 GPa Show Material materials with Elastic modulus of 200 GPa |
Elongation | 20.0 °C | 25 % Show Material materials with Elongation of 25 % |
Hardness, Brinell | 20.0 °C | 230 [-] Show Material materials with Hardness, Brinell of 230 [-] |
Tensile strength | 20.0 °C | 600 MPa Show Material materials with Tensile strength of 600 MPa |
Yield strength Rp0.2 | 20.0 °C | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa |
Yield strength Rp1.0 | 20.0 °C | 250 MPa Show Material materials with Yield strength Rp1.0 of 250 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K | |
200.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
400.0 °C | 1.5E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.5E-5 1/K | ||
600.0 °C | 1.55E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.55E-5 1/K | ||
800.0 °C | 1.6E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K | ||
Max service temperature, long | 0 - 1150 °C Show Material materials with Max service temperature, long of 0 - 1150 °C | ||
Melting point | 1400 °C Show Material materials with Melting point of 1400 °C | Typical for Nickel Chromium Alloy | |
Specific heat capacity | 20.0 °C | 460 J/(kg·K) Show Material materials with Specific heat capacity of 460 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 13 W/(m·K) Show Material materials with Thermal conductivity of 13 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m |
100.0 °C | 1.14E-6 Ω·m Show Material materials with Electrical resistivity of 1.14E-6 Ω·m | |
200.0 °C | 1.16E-6 Ω·m Show Material materials with Electrical resistivity of 1.16E-6 Ω·m | |
300.0 °C | 1.18E-6 Ω·m Show Material materials with Electrical resistivity of 1.18E-6 Ω·m | |
400.0 °C | 1.2E-6 Ω·m Show Material materials with Electrical resistivity of 1.2E-6 Ω·m | |
500.0 °C | 1.22E-6 Ω·m Show Material materials with Electrical resistivity of 1.22E-6 Ω·m | |
600.0 °C | 1.21E-6 Ω·m Show Material materials with Electrical resistivity of 1.21E-6 Ω·m | |
700.0 °C | 1.21E-6 Ω·m Show Material materials with Electrical resistivity of 1.21E-6 Ω·m | |
800.0 °C | 1.22E-6 Ω·m Show Material materials with Electrical resistivity of 1.22E-6 Ω·m | |
900.0 °C | 1.23E-6 Ω·m Show Material materials with Electrical resistivity of 1.23E-6 Ω·m | |
1000.0 °C | 1.24E-6 Ω·m Show Material materials with Electrical resistivity of 1.24E-6 Ω·m | |
1100.0 °C | 1.26E-6 Ω·m Show Material materials with Electrical resistivity of 1.26E-6 Ω·m | |
1200.0 °C | 1.28E-6 Ω·m Show Material materials with Electrical resistivity of 1.28E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.3 % Show Material materials with Aluminium of 0.3 % |
Carbon | 0.15 % Show Material materials with Carbon of 0.15 % |
Chromium | 19 - 21 % Show Material materials with Chromium of 19 - 21 % |
Copper | 0.5 % Show Material materials with Copper of 0.5 % |
Iron | 1 % Show Material materials with Iron of 1 % |
Manganese | 1 % Show Material materials with Manganese of 1 % |
Nickel | 75 % Show Material materials with Nickel of 75 % |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % |
Silicon | 0.5 - 2 % Show Material materials with Silicon of 0.5 - 2 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |