Description

The material NiCr22Mo7Cu with the material number 2.4619 is applied for corrosion-resistant construction components in the form of strips, sheets, tubes, bars, wires and forgings. It is a further development of the material NiCr22Mo6Cu (material number 2.4618) and has an excellent resistant to pitting, crevice and stress cracking corrosion. The alloy is of good weldability and possesses good resistance to intergranular corrosion in the welded condition. The low carbon content prevents sensitizing and its results, i.e. intergranular corrosion of the heat affected zone of the welding seams. The material is oustandingly resistant to strongly corroding chloride- and fluoride-polluted sulphuric and phosphoric acid. Application for plants for the production and processing of sulphuric, phosphoric and nitric acid. For components in flue-gas desulphurization and waste incineration plants, in the paper and cellulose industry and for the extraction of acid gas. Processing properties: Formability: good Weldability: good

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.3 g/cm³

Show Material materials with Density of 8.3 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

211 GPa

Show Material materials with Elastic modulus of 211 GPa

100.0 °C

205 GPa

Show Material materials with Elastic modulus of 205 GPa

200.0 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

300.0 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

400.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

173 GPa

Show Material materials with Elastic modulus of 173 GPa

700.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

Elongation

20.0 °C

35 - 45 %

Show Material materials with Elongation of 35 - 45 %

100.0 °C

60 %

Show Material materials with Elongation of 60 %

200.0 °C

60 %

Show Material materials with Elongation of 60 %

300.0 °C

65 %

Show Material materials with Elongation of 65 %

400.0 °C

65 %

Show Material materials with Elongation of 65 %

500.0 °C

65 %

Show Material materials with Elongation of 65 %

600.0 °C

65 %

Show Material materials with Elongation of 65 %

Unlock all property charts

Hardness, Brinell

20.0 °C

240 [-]

Show Material materials with Hardness, Brinell of 240 [-]

Tensile strength

20.0 °C

585 - 620 MPa

Show Material materials with Tensile strength of 585 - 620 MPa

100.0 °C

640 MPa

Show Material materials with Tensile strength of 640 MPa

200.0 °C

590 MPa

Show Material materials with Tensile strength of 590 MPa

300.0 °C

570 MPa

Show Material materials with Tensile strength of 570 MPa

400.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

500.0 °C

530 MPa

Show Material materials with Tensile strength of 530 MPa

600.0 °C

500 MPa

Show Material materials with Tensile strength of 500 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

205 - 240 MPa

Show Material materials with Yield strength Rp0.2 of 205 - 240 MPa

100.0 °C

270 MPa

Show Material materials with Yield strength Rp0.2 of 270 MPa

200.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

300.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

400.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

500.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

600.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

Unlock all property charts

Yield strength Rp1.0

20.0 °C

225 - 260 MPa

Show Material materials with Yield strength Rp1.0 of 225 - 260 MPa

100.0 °C

290 MPa

Show Material materials with Yield strength Rp1.0 of 290 MPa

200.0 °C

260 MPa

Show Material materials with Yield strength Rp1.0 of 260 MPa

300.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

400.0 °C

220 MPa

Show Material materials with Yield strength Rp1.0 of 220 MPa

500.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

600.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0 of 200 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.43E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.43E-5 1/K

200.0 °C

1.47E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.47E-5 1/K

300.0 °C

1.5E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.5E-5 1/K

400.0 °C

1.53E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.53E-5 1/K

500.0 °C

1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 1/K

600.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

700.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

Unlock all property charts

Melting point

1400 °C

Show Material materials with Melting point of 1400 °C

Typical for Nickel Chromium Alloy

Specific heat capacity

20.0 °C

441 J/(kg·K)

Show Material materials with Specific heat capacity of 441 J/(kg·K)

100.0 °C

452 J/(kg·K)

Show Material materials with Specific heat capacity of 452 J/(kg·K)

200.0 °C

462 J/(kg·K)

Show Material materials with Specific heat capacity of 462 J/(kg·K)

300.0 °C

471 J/(kg·K)

Show Material materials with Specific heat capacity of 471 J/(kg·K)

400.0 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

500.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

600.0 °C

495 J/(kg·K)

Show Material materials with Specific heat capacity of 495 J/(kg·K)

700.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

10 W/(m·K)

Show Material materials with Thermal conductivity of 10 W/(m·K)

100.0 °C

12.6 W/(m·K)

Show Material materials with Thermal conductivity of 12.6 W/(m·K)

200.0 °C

14.3 W/(m·K)

Show Material materials with Thermal conductivity of 14.3 W/(m·K)

300.0 °C

16 W/(m·K)

Show Material materials with Thermal conductivity of 16 W/(m·K)

400.0 °C

17.7 W/(m·K)

Show Material materials with Thermal conductivity of 17.7 W/(m·K)

500.0 °C

19.3 W/(m·K)

Show Material materials with Thermal conductivity of 19.3 W/(m·K)

600.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

700.0 °C

22.6 W/(m·K)

Show Material materials with Thermal conductivity of 22.6 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

100.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

200.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

300.0 °C

1.21E-6 Ω·m

Show Material materials with Electrical resistivity of 1.21E-6 Ω·m

400.0 °C

1.23E-6 Ω·m

Show Material materials with Electrical resistivity of 1.23E-6 Ω·m

500.0 °C

1.25E-6 Ω·m

Show Material materials with Electrical resistivity of 1.25E-6 Ω·m

600.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

700.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.015 %

Show Material materials with Carbon of 0.015 %

Chromium

21 - 23.5 %

Show Material materials with Chromium of 21 - 23.5 %

Cobalt

5 %

Show Material materials with Cobalt of 5 %

Copper

1.5 - 2.5 %

Show Material materials with Copper of 1.5 - 2.5 %

Iron

18 - 21 %

Show Material materials with Iron of 18 - 21 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

6 - 8 %

Show Material materials with Molybdenum of 6 - 8 %

Nickel

35.95 %

Show Material materials with Nickel of 35.95 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Tungsten

1.5 %