DIN 17744 Grade NiMo16Cr15W solution heat-treated and quenched

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.9 g/cm³

Show Material materials with Density of 8.9 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

208 GPa

Show Material materials with Elastic modulus of 208 GPa

100.0 °C

204 GPa

Show Material materials with Elastic modulus of 204 GPa

200.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

300.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

400.0 °C

188 GPa

Show Material materials with Elastic modulus of 188 GPa

500.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

600.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

700.0 °C

168 GPa

Show Material materials with Elastic modulus of 168 GPa

800.0 °C

160 GPa

Show Material materials with Elastic modulus of 160 GPa

900.0 °C

151 GPa

Show Material materials with Elastic modulus of 151 GPa

1000.0 °C

143 GPa

Show Material materials with Elastic modulus of 143 GPa

Elongation

20.0 °C

25 - 35 %

Show Material materials with Elongation of 25 - 35 %

Tensile strength

20.0 °C

700 - 1000 MPa

Show Material materials with Tensile strength of 700 - 1000 MPa

Yield strength Rp0.2

20.0 °C

280 - 310 MPa

Show Material materials with Yield strength Rp0.2 of 280 - 310 MPa

100.0 °C

255 - 280 MPa

Show Material materials with Yield strength Rp0.2 of 255 - 280 MPa

200.0 °C

225 - 240 MPa

Show Material materials with Yield strength Rp0.2 of 225 - 240 MPa

300.0 °C

200 - 220 MPa

Show Material materials with Yield strength Rp0.2 of 200 - 220 MPa

400.0 °C

170 - 195 MPa

Show Material materials with Yield strength Rp0.2 of 170 - 195 MPa

450.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2 of 150 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

100.0 °C

255 - 280 MPa

Show Material materials with Yield strength Rp0.2, transverse of 255 - 280 MPa

200.0 °C

225 - 240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 225 - 240 MPa

300.0 °C

200 - 220 MPa

Show Material materials with Yield strength Rp0.2, transverse of 200 - 220 MPa

400.0 °C

170 - 195 MPa

Show Material materials with Yield strength Rp0.2, transverse of 170 - 195 MPa

450.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2, transverse of 150 MPa

Unlock all property charts

Yield strength Rp1.0

20.0 °C

300 - 330 MPa

Show Material materials with Yield strength Rp1.0 of 300 - 330 MPa

100.0 °C

275 - 305 MPa

Show Material materials with Yield strength Rp1.0 of 275 - 305 MPa

200.0 °C

245 - 275 MPa

Show Material materials with Yield strength Rp1.0 of 245 - 275 MPa

300.0 °C

215 - 245 MPa

Show Material materials with Yield strength Rp1.0 of 215 - 245 MPa

400.0 °C

200 - 230 MPa

Show Material materials with Yield strength Rp1.0 of 200 - 230 MPa

450.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

100.0 °C

275 - 305 MPa

Show Material materials with Yield strength Rp1.0, transverse of 275 - 305 MPa

200.0 °C

245 - 275 MPa

Show Material materials with Yield strength Rp1.0, transverse of 245 - 275 MPa

300.0 °C

215 - 245 MPa

Show Material materials with Yield strength Rp1.0, transverse of 215 - 245 MPa

400.0 °C

200 - 230 MPa

Show Material materials with Yield strength Rp1.0, transverse of 200 - 230 MPa

450.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0, transverse of 160 MPa

Unlock all property charts

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.17E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.17E-5 1/K

200.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

300.0 °C

1.28E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.28E-5 1/K

400.0 °C

1.31E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.31E-5 1/K

500.0 °C

1.35E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K

600.0 °C

1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K

700.0 °C

1.47E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.47E-5 1/K

800.0 °C

1.55E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.55E-5 1/K

900.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

1000.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

Unlock all property charts

Specific heat capacity

20.0 °C

407 - 426 J/(kg·K)

Show Material materials with Specific heat capacity of 407 - 426 J/(kg·K)

100.0 °C

430 - 438 J/(kg·K)

Show Material materials with Specific heat capacity of 430 - 438 J/(kg·K)

200.0 °C

453 - 454 J/(kg·K)

Show Material materials with Specific heat capacity of 453 - 454 J/(kg·K)

300.0 °C

469 - 474 J/(kg·K)

Show Material materials with Specific heat capacity of 469 - 474 J/(kg·K)

400.0 °C

483 - 492 J/(kg·K)

Show Material materials with Specific heat capacity of 483 - 492 J/(kg·K)

500.0 °C

493 - 503 J/(kg·K)

Show Material materials with Specific heat capacity of 493 - 503 J/(kg·K)

600.0 °C

515 - 517 J/(kg·K)

Show Material materials with Specific heat capacity of 515 - 517 J/(kg·K)

700.0 °C

527 - 609 J/(kg·K)

Show Material materials with Specific heat capacity of 527 - 609 J/(kg·K)

800.0 °C

536 - 605 J/(kg·K)

Show Material materials with Specific heat capacity of 536 - 605 J/(kg·K)

900.0 °C

545 - 609 J/(kg·K)

Show Material materials with Specific heat capacity of 545 - 609 J/(kg·K)

1000.0 °C

551 - 605 J/(kg·K)

Show Material materials with Specific heat capacity of 551 - 605 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

10.2 - 10.6 W/(m·K)

Show Material materials with Thermal conductivity of 10.2 - 10.6 W/(m·K)

100.0 °C

11.6 - 12 W/(m·K)

Show Material materials with Thermal conductivity of 11.6 - 12 W/(m·K)

200.0 °C

13.4 - 13.7 W/(m·K)

Show Material materials with Thermal conductivity of 13.4 - 13.7 W/(m·K)

300.0 °C

15.1 - 15.4 W/(m·K)

Show Material materials with Thermal conductivity of 15.1 - 15.4 W/(m·K)

400.0 °C

16.7 - 17.1 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 - 17.1 W/(m·K)

500.0 °C

18.1 - 18.7 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 - 18.7 W/(m·K)

600.0 °C

20.2 - 20.7 W/(m·K)

Show Material materials with Thermal conductivity of 20.2 - 20.7 W/(m·K)

700.0 °C

22.6 - 25.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.6 - 25.7 W/(m·K)

800.0 °C

24.3 - 25.8 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 - 25.8 W/(m·K)

900.0 °C

25.9 - 26.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 - 26.2 W/(m·K)

1000.0 °C

27.2 - 28 W/(m·K)

Show Material materials with Thermal conductivity of 27.2 - 28 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.25E-6 Ω·m

Show Material materials with Electrical resistivity of 1.25E-6 Ω·m

100.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

200.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

300.0 °C

1.29E-6 Ω·m

Show Material materials with Electrical resistivity of 1.29E-6 Ω·m

400.0 °C

1.3E-6 Ω·m

Show Material materials with Electrical resistivity of 1.3E-6 Ω·m

500.0 °C

1.29E-6 Ω·m

Show Material materials with Electrical resistivity of 1.29E-6 Ω·m

600.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

700.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

800.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.01 %

Show Material materials with Carbon of 0.01 %

Chromium

14.5 - 16.5 %

Show Material materials with Chromium of 14.5 - 16.5 %

Cobalt

2.5 %

Show Material materials with Cobalt of 2.5 %

Iron

4 - 7 %

Show Material materials with Iron of 4 - 7 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

15 - 17 %

Show Material materials with Molybdenum of 15 - 17 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.08 %

Show Material materials with Silicon of 0.08 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

Tungsten

3 - 4.5 %

Show Material materials with Tungsten of 3 - 4.5 %

Vanadium

0.35 %

Show Material materials with Vanadium of 0.35 %