DIN 17744 Grade NiMo16Cr16Ti solution heat-treated and quenched

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.6 - 8.7 g/cm³

Show Material materials with Density of 8.6 - 8.7 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

211 GPa

Show Material materials with Elastic modulus of 211 GPa

100.0 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

200.0 °C

202 GPa

Show Material materials with Elastic modulus of 202 GPa

300.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

400.0 °C

188 GPa

Show Material materials with Elastic modulus of 188 GPa

500.0 °C

181 GPa

Show Material materials with Elastic modulus of 181 GPa

600.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

700.0 °C

168 GPa

Show Material materials with Elastic modulus of 168 GPa

800.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

900.0 °C

149 GPa

Show Material materials with Elastic modulus of 149 GPa

1000.0 °C

138 GPa

Show Material materials with Elastic modulus of 138 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation A80

20.0 °C

40 %

Show Material materials with Elongation A80 of 40 %

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

40 %

Show Material materials with Elongation, transverse of 40 %

Tensile strength

20.0 °C

700 - 900 MPa

Show Material materials with Tensile strength of 700 - 900 MPa

Tensile strength, transverse

20.0 °C

700 - 900 MPa

Show Material materials with Tensile strength, transverse of 700 - 900 MPa

Yield strength Rp0.2

20.0 °C

280 - 305 MPa

Show Material materials with Yield strength Rp0.2 of 280 - 305 MPa

100.0 °C

260 - 285 MPa

Show Material materials with Yield strength Rp0.2 of 260 - 285 MPa

200.0 °C

235 - 255 MPa

Show Material materials with Yield strength Rp0.2 of 235 - 255 MPa

300.0 °C

215 - 245 MPa

Show Material materials with Yield strength Rp0.2 of 215 - 245 MPa

400.0 °C

205 - 225 MPa

Show Material materials with Yield strength Rp0.2 of 205 - 225 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

280 - 305 MPa

Show Material materials with Yield strength Rp0.2, transverse of 280 - 305 MPa

100.0 °C

260 - 285 MPa

Show Material materials with Yield strength Rp0.2, transverse of 260 - 285 MPa

200.0 °C

235 - 255 MPa

Show Material materials with Yield strength Rp0.2, transverse of 235 - 255 MPa

300.0 °C

215 - 245 MPa

Show Material materials with Yield strength Rp0.2, transverse of 215 - 245 MPa

400.0 °C

205 - 225 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 - 225 MPa

Unlock all property charts

Yield strength Rp1.0

20.0 °C

315 - 340 MPa

Show Material materials with Yield strength Rp1.0 of 315 - 340 MPa

100.0 °C

295 - 315 MPa

Show Material materials with Yield strength Rp1.0 of 295 - 315 MPa

200.0 °C

275 - 285 MPa

Show Material materials with Yield strength Rp1.0 of 275 - 285 MPa

300.0 °C

255 - 270 MPa

Show Material materials with Yield strength Rp1.0 of 255 - 270 MPa

400.0 °C

240 - 260 MPa

Show Material materials with Yield strength Rp1.0 of 240 - 260 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

315 - 340 MPa

Show Material materials with Yield strength Rp1.0, transverse of 315 - 340 MPa

100.0 °C

295 - 315 MPa

Show Material materials with Yield strength Rp1.0, transverse of 295 - 315 MPa

200.0 °C

275 - 285 MPa

Show Material materials with Yield strength Rp1.0, transverse of 275 - 285 MPa

300.0 °C

255 - 270 MPa

Show Material materials with Yield strength Rp1.0, transverse of 255 - 270 MPa

400.0 °C

240 - 260 MPa

Show Material materials with Yield strength Rp1.0, transverse of 240 - 260 MPa

Unlock all property charts

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.09E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 1/K

200.0 °C

1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K

300.0 °C

1.25E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K

400.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

500.0 °C

1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K

600.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

700.0 °C

1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K

800.0 °C

1.45E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K

900.0 °C

1.51E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.51E-5 1/K

1000.0 °C

1.59E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.59E-5 1/K

Unlock all property charts

Specific heat capacity

20.0 °C

408 J/(kg·K)

Show Material materials with Specific heat capacity of 408 J/(kg·K)

100.0 °C

426 J/(kg·K)

Show Material materials with Specific heat capacity of 426 J/(kg·K)

200.0 °C

448 J/(kg·K)

Show Material materials with Specific heat capacity of 448 J/(kg·K)

300.0 °C

465 J/(kg·K)

Show Material materials with Specific heat capacity of 465 J/(kg·K)

400.0 °C

477 J/(kg·K)

Show Material materials with Specific heat capacity of 477 J/(kg·K)

500.0 °C

490 J/(kg·K)

Show Material materials with Specific heat capacity of 490 J/(kg·K)

600.0 °C

502 J/(kg·K)

Show Material materials with Specific heat capacity of 502 J/(kg·K)

700.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

800.0 °C

522 J/(kg·K)

Show Material materials with Specific heat capacity of 522 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

10.1 W/(m·K)

Show Material materials with Thermal conductivity of 10.1 W/(m·K)

100.0 °C

11.4 W/(m·K)

Show Material materials with Thermal conductivity of 11.4 W/(m·K)

200.0 °C

13.2 W/(m·K)

Show Material materials with Thermal conductivity of 13.2 W/(m·K)

300.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

400.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

500.0 °C

18.4 W/(m·K)

Show Material materials with Thermal conductivity of 18.4 W/(m·K)

600.0 °C

20.5 W/(m·K)

Show Material materials with Thermal conductivity of 20.5 W/(m·K)

700.0 °C

22.6 W/(m·K)

Show Material materials with Thermal conductivity of 22.6 W/(m·K)

800.0 °C

24.8 W/(m·K)

Show Material materials with Thermal conductivity of 24.8 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

100.0 °C

1.25E-6 Ω·m

Show Material materials with Electrical resistivity of 1.25E-6 Ω·m

200.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

300.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

400.0 °C

1.28E-6 Ω·m

Show Material materials with Electrical resistivity of 1.28E-6 Ω·m

500.0 °C

1.29E-6 Ω·m

Show Material materials with Electrical resistivity of 1.29E-6 Ω·m

600.0 °C

1.32E-6 Ω·m

Show Material materials with Electrical resistivity of 1.32E-6 Ω·m

700.0 °C

1.35E-6 Ω·m

Show Material materials with Electrical resistivity of 1.35E-6 Ω·m

800.0 °C

1.38E-6 Ω·m

Show Material materials with Electrical resistivity of 1.38E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

9E-3 %

Show Material materials with Carbon of 9E-3 %

Chromium

14.5 - 17.5 %

Show Material materials with Chromium of 14.5 - 17.5 %

Cobalt

2 %

Show Material materials with Cobalt of 2 %

Iron

3 %

Show Material materials with Iron of 3 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

14 - 17 %

Show Material materials with Molybdenum of 14 - 17 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.05 %

Show Material materials with Silicon of 0.05 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

Titanium

0.7 %

Show Material materials with Titanium of 0.7 %