General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 7.15 g/cm³ Show Material materials with Density of 7.15 g/cm³ | Typical for Ductile (Nodular) Cast Iron |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Compressive yield strength | 20.0 °C | 800 MPa Show Material materials with Compressive yield strength of 800 MPa | |
Elastic modulus | 23.0 °C | 165 - 180 GPa Show Material materials with Elastic modulus of 165 - 180 GPa | Typical for Ductile (Nodular) Cast Iron |
Elongation | 20.0 °C | 7 % Show Material materials with Elongation of 7 % | |
Hardness, Brinell | 20.0 °C | 170 - 220 [-] Show Material materials with Hardness, Brinell of 170 - 220 [-] | |
Poisson's ratio | 20.0 °C | 0.27 - 0.29 [-] Show Material materials with Poisson's ratio of 0.27 - 0.29 [-] | |
Shear modulus | 23.0 °C | 63 - 66 GPa Show Material materials with Shear modulus of 63 - 66 GPa | Typical for Ductile (Nodular) Cast Iron |
Tensile strength | 20.0 °C | 500 MPa Show Material materials with Tensile strength of 500 MPa | |
Yield strength | 20.0 °C | 320 MPa Show Material materials with Yield strength of 320 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K | |
200.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | ||
300.0 °C | 1.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K | ||
400.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K | ||
Melting point | 1150 - 1200 °C Show Material materials with Melting point of 1150 - 1200 °C | Typical for Ductile (Nodular) Cast Iron | |
Specific heat capacity | 23.0 °C | 460 - 502 J/(kg·K) Show Material materials with Specific heat capacity of 460 - 502 J/(kg·K) | Typical for Ductile (Nodular) Cast Iron |
Thermal conductivity | 100.0 °C | 33 W/(m·K) Show Material materials with Thermal conductivity of 33 W/(m·K) | |
200.0 °C | 34 W/(m·K) Show Material materials with Thermal conductivity of 34 W/(m·K) | ||
300.0 °C | 33 W/(m·K) Show Material materials with Thermal conductivity of 33 W/(m·K) | ||
400.0 °C | 32 W/(m·K) Show Material materials with Thermal conductivity of 32 W/(m·K) | ||
500.0 °C | 30 W/(m·K) Show Material materials with Thermal conductivity of 30 W/(m·K) | ||
Chemical properties
Property | Value |
---|---|
Carbon | 3.5 - 3.8 % Show Material materials with Carbon of 3.5 - 3.8 % |
Magnesium | 0.06 - 0.12 % Show Material materials with Magnesium of 0.06 - 0.12 % |
Manganese | 0.4 % Show Material materials with Manganese of 0.4 % |
Phosphorus | 0.1 % Show Material materials with Phosphorus of 0.1 % |
Silicon | 2 - 3 % Show Material materials with Silicon of 2 - 3 % |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.