General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 6.8 - 7.8 g/cm³ Show Material materials with Density of 6.8 - 7.8 g/cm³ | Typical for Cast Iron |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 152 GPa Show Material materials with Elastic modulus of 152 GPa | Typical for Cast Iron |
Hardness, Brinell | 23.0 °C | 400 [-] Show Material materials with Hardness, Brinell of 400 [-] | |
Hardness, Rockwell C | 23.0 °C | 41 [-] Show Material materials with Hardness, Rockwell C of 41 [-] | |
Hardness, Vickers | 23.0 °C | 430 [-] Show Material materials with Hardness, Vickers of 430 [-] | |
Poisson's ratio | 23.0 °C | 0.27 [-] Show Material materials with Poisson's ratio of 0.27 [-] | Typical for Cast Iron |
Shear modulus | 23.0 °C | 41 GPa Show Material materials with Shear modulus of 41 GPa | Typical for Cast Iron |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Melting point | 1120 °C Show Material materials with Melting point of 1120 °C | Typical for Cast Iron | |
Specific heat capacity | 23.0 °C | 460 - 527 J/(kg·K) Show Material materials with Specific heat capacity of 460 - 527 J/(kg·K) | Typical for Cast Iron |
Thermal conductivity | 23.0 °C | 55 W/(m·K) Show Material materials with Thermal conductivity of 55 W/(m·K) | Typical for Cast Iron |
Chemical properties
Property | Value |
---|---|
Carbon | 2 - 3.3 % Show Material materials with Carbon of 2 - 3.3 % |
Chromium | 14 - 18 % Show Material materials with Chromium of 14 - 18 % |
Copper | 1.2 % Show Material materials with Copper of 1.2 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Molybdenum | 3 % Show Material materials with Molybdenum of 3 % |
Nickel | 2.5 % Show Material materials with Nickel of 2.5 % |
Phosphorus | 0.1 % Show Material materials with Phosphorus of 0.1 % |
Silicon | 1.5 % Show Material materials with Silicon of 1.5 % |
Sulfur | 0.06 % Show Material materials with Sulfur of 0.06 % |