General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 2.1 g/cm³ Show Material materials with Density of 2.1 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 45 GPa Show Material materials with Elastic modulus of 45 GPa | |
Elongation | 23.0 °C | 4.6 - 10 % Show Material materials with Elongation of 4.6 - 10 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Magnesium |
Shear modulus | 23.0 °C | 45 GPa Show Material materials with Shear modulus of 45 GPa | Typical for Magnesium |
Tensile strength | 23.0 °C | 320 - 340 MPa Show Material materials with Tensile strength of 320 - 340 MPa | |
Yield strength | 23.0 °C | 230 - 250 MPa Show Material materials with Yield strength of 230 - 250 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.6E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.6E-5 1/K |
Melting point | 550 °C Show Material materials with Melting point of 550 °C | |
Specific heat capacity | 23.0 °C | 990 J/(kg·K) Show Material materials with Specific heat capacity of 990 J/(kg·K) |
Thermal conductivity | 23.0 °C | 81 W/(m·K) Show Material materials with Thermal conductivity of 81 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Magnesium | 92.5 - 94.8 % Show Material materials with Magnesium of 92.5 - 94.8 % |
Other | 0 - 0.3 % Show Material materials with Other of 0 - 0.3 % |
Zinc | 4.8 - 6.2 % Show Material materials with Zinc of 4.8 - 6.2 % |
Zirconium | 0.45 - 1 % Show Material materials with Zirconium of 0.45 - 1 % |