ZK61A

Want to keep this datasheet? Save it now in your required format

This material data has been provided by MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueTemperature

Density

2.1 g/cm³

Show Material materials with Density of 2.1 g/cm³ at 23.0 °C

23.0 °C

Mechanical

PropertyValueTemperatureComment

Elastic modulus

49 GPa

Show Material materials with Elastic modulus of 49 GPa at 23.0 °C

23.0 °C

Elongation

5.8 - 7.2 %

Show Material materials with Elongation of 5.8 - 7.2 % at 23.0 °C

23.0 °C

Poisson's ratio

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-] at 23.0 °C

23.0 °C

Typical for Magnesium

Shear modulus

45 GPa

Show Material materials with Shear modulus of 45 GPa at 23.0 °C

23.0 °C

Typical for Magnesium

Tensile strength

290 - 310 MPa

Show Material materials with Tensile strength of 290 - 310 MPa at 23.0 °C

23.0 °C

Yield strength

180 - 200 MPa

Show Material materials with Yield strength of 180 - 200 MPa at 23.0 °C

23.0 °C

Thermal

PropertyValueTemperatureComment

Coefficient of thermal expansion

2.5E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.5E-5 1/K at 23.0 °C

23.0 °C

Melting point

530 °C

Show Material materials with Melting point of 530 °C

Specific heat capacity

960 J/(kg·K)

Show Material materials with Specific heat capacity of 960 J/(kg·K) at 23.0 °C

23.0 °C

Thermal conductivity

153 - 167 W/(m·K)

Show Material materials with Thermal conductivity of 153 - 167 W/(m·K) at 23.0 °C

23.0 °C

Typical for Magnesium

Chemical properties

Property

Copper

0 - 0.1 %

Magnesium

92.1 - 93.9 %

Nickel

0 - 0.01 %

Other

0 - 0.3 %

Zinc

5.5 - 6.5 %

Zirconium

0.6 - 1 %