ASTM Grade 9 Annealed

Alternative and trade names
Ti-3Al-2.5V
Want to keep this datasheet? Save it now in your required format

Description

Titanium ASTM Grade 9 has medium strength that falls between Grade 4 and Grade 5. It has excellent corrosion resistance and is used in Aerospace and Industrial applications. ASTM Grade 9 Titanium can be used at higher temperatures than Grades 1 through 4. ASTM Grade 9 titanium has good cold rolling properties.

Equivalent Materials

This material data has been provided by MakeItFrom.com,NIPPON.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueCondition

Density

4.5 g/cm³

Show Material materials with Density of 4.5 g/cm³

Annealed

Mechanical

PropertyValueConditionShape

Elastic modulus

110.0 GPa

Show Material materials with Elastic modulus of 110.0 GPa

Annealed

Elongation

17.0 %

Show Material materials with Elongation of 17.0 %

Annealed

Tensile strength

710.0 MPa

Show Material materials with Tensile strength of 710.0 MPa

Annealed

620.0 MPa

Show Material materials with Tensile strength of 620.0 MPa

Annealed

Sheet, Welded tube, bar

Yield strength

560.0 MPa

Show Material materials with Yield strength of 560.0 MPa

Annealed

483.0 MPa

Show Material materials with Yield strength of 483.0 MPa

Annealed

Sheet, Welded tube, bar

Thermal

PropertyValueConditionComment

Coefficient of thermal expansion

9.1e-06 1/K

Show Material materials with Coefficient of thermal expansion of 9.1e-06 1/K

Annealed

Melting point

1668.0 °C

Show Material materials with Melting point of 1668.0 °C

Typical for Titanium

Specific heat capacity

490.0 J/(kg·K)

Show Material materials with Specific heat capacity of 490.0 J/(kg·K)

Annealed

Thermal conductivity

8.1 W/(m·K)

Show Material materials with Thermal conductivity of 8.1 W/(m·K)

Annealed

Chemical properties

PropertyValueConditionShape

Aluminium

2.5 - 3.5 %

Show Material materials with Aluminium of 2.5 - 3.5 %

Annealed

2.5 - 3.0 %

Show Material materials with Aluminium of 2.5 - 3.0 %

Annealed

Sheet, Welded tube, bar

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Annealed

Sheet, Welded tube, bar

Hydrogen

0.015 %

Show Material materials with Hydrogen of 0.015 %

Annealed

Iron

0.25 %

Show Material materials with Iron of 0.25 %

Annealed

Sheet, Welded tube, bar

Nitrogen

0.03 %

Show Material materials with Nitrogen of 0.03 %

Annealed

Sheet, Welded tube, bar

Other

0.4 %

Show Material materials with Other of 0.4 %

Annealed

Oxygen

0.15 %

Show Material materials with Oxygen of 0.15 %

Annealed

Sheet, Welded tube, bar

Titanium

92.6 - 95.5 %

Show Material materials with Titanium of 92.6 - 95.5 %

Annealed

Vanadium

2.0 - 3.0 %

Show Material materials with Vanadium of 2.0 - 3.0 %

Annealed

Sheet, Welded tube, bar