General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 4.505 g/cm³ Show Material materials with Density of 4.505 g/cm³ | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 108.0 GPa Show Material materials with Elastic modulus of 108.0 GPa | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | |
200.0 °C | 95.0 GPa Show Material materials with Elastic modulus of 95.0 GPa | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | ||
400.0 °C | 81.0 GPa Show Material materials with Elastic modulus of 81.0 GPa | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | ||
Poisson's ratio | 0.361 [-] Show Material materials with Poisson's ratio of 0.361 [-] | Typical for Pure Titanium | ||||
Shear modulus | 46.0 GPa Show Material materials with Shear modulus of 46.0 GPa | Typical for Pure Titanium | ||||
Tensile strength | 20.0 °C | 690.0 MPa Show Material materials with Tensile strength of 690.0 MPa | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 8.400000000000001e-06 - 8.599999999999999e-06 1/K Show Material materials with Coefficient of thermal expansion of 8.400000000000001e-06 - 8.599999999999999e-06 1/K | Typical for Pure Titanium | ||||
Melting point | 1670.0 °C Show Material materials with Melting point of 1670.0 °C | Typical for Pure Titanium | ||||
Specific heat capacity | 20.0 °C | 540.0 J/(kg·K) Show Material materials with Specific heat capacity of 540.0 J/(kg·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Specific heat capacity of 570.0 J/(kg·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Specific heat capacity of 630.0 J/(kg·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | ||
Thermal conductivity | 20.0 °C | 20.1 W/(m·K) Show Material materials with Thermal conductivity of 20.1 W/(m·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | |
200.0 °C | 20.1 W/(m·K) Show Material materials with Thermal conductivity of 20.1 W/(m·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Thermal conductivity of 20.5 W/(m·K) | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | 20.0 °C | 5.5e-07 Ω·m Show Material materials with Electrical resistivity of 5.5e-07 Ω·m | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
200.0 °C | 8.8e-07 Ω·m Show Material materials with Electrical resistivity of 8.8e-07 Ω·m | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire | |
400.0 °C | 1.22e-06 Ω·m Show Material materials with Electrical resistivity of 1.22e-06 Ω·m | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.06 Show Material materials with Carbon of 0.06 | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Hydrogen | 0.013 Show Material materials with Hydrogen of 0.013 | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Iron | 0.3 Show Material materials with Iron of 0.3 | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Nitrogen | 0.05 Show Material materials with Nitrogen of 0.05 | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Oxygen | 0.35 Show Material materials with Oxygen of 0.35 | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |
Titanium | 98.8 % Show Material materials with Titanium of 98.8 % | 1/2 Hard | DIN 17850, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Wire |