General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 4.505 g/cm³ Show Material materials with Density of 4.505 g/cm³ | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 108.0 - 110.0 GPa Show Material materials with Elastic modulus of 108.0 - 110.0 GPa | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
200.0 °C | 96.0 - 97.0 GPa Show Material materials with Elastic modulus of 96.0 - 97.0 GPa | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | |
400.0 °C | 82.0 GPa Show Material materials with Elastic modulus of 82.0 GPa | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 7.599999999999997e-06 - 1.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Near Alpha Alloy | ||||
Melting point | 1540.0 - 1715.0 °C Show Material materials with Melting point of 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy | ||||
Specific heat capacity | 20.0 °C | 520.0 J/(kg·K) Show Material materials with Specific heat capacity of 520.0 J/(kg·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Specific heat capacity of 570.0 J/(kg·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Specific heat capacity of 630.0 J/(kg·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | ||
Thermal conductivity | 20.0 °C | 22.6 W/(m·K) Show Material materials with Thermal conductivity of 22.6 W/(m·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | |
200.0 °C | 20.9 W/(m·K) Show Material materials with Thermal conductivity of 20.9 W/(m·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | ||
400.0 °C | 19.3 W/(m·K) Show Material materials with Thermal conductivity of 19.3 W/(m·K) | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | 20.0 °C | 5.2e-07 Ω·m Show Material materials with Electrical resistivity of 5.2e-07 Ω·m | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
200.0 °C | 8.7e-07 Ω·m Show Material materials with Electrical resistivity of 8.7e-07 Ω·m | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat | |
400.0 °C | 1.2e-06 Ω·m Show Material materials with Electrical resistivity of 1.2e-06 Ω·m | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.06 Show Material materials with Carbon of 0.06 | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Hydrogen | 0.013 Show Material materials with Hydrogen of 0.013 | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Iron | 0.25 Show Material materials with Iron of 0.25 | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Molybdenum | 0.2 - 0.4 % Show Material materials with Molybdenum of 0.2 - 0.4 % | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Nickel | 0.6 - 0.9 % Show Material materials with Nickel of 0.6 - 0.9 % | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Nitrogen | 0.03 Show Material materials with Nitrogen of 0.03 | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Oxygen | 0.25 Show Material materials with Oxygen of 0.25 | Welded | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Tube, Flat |
Titanium | 97.7 % Show Material materials with Titanium of 97.7 % | Welded | DIN 17851, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-3 | Tube |