General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 4.56 g/cm³ Show Material materials with Density of 4.56 g/cm³ | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 113.0 GPa Show Material materials with Elastic modulus of 113.0 GPa | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Elongation | 20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | Annealed | WL 3.7124-1 | Forging, Rod |
Reduction of area | 20.0 °C | 35.0 Show Material materials with Reduction of area of 35.0 | Annealed | WL 3.7124-1 | Forging, Rod |
Tensile strength | 20.0 °C | 540.0 MPa Show Material materials with Tensile strength of 540.0 MPa | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 7.599999999999997e-06 - 1.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Alpha Alloy |
Melting point | 1540.0 - 1715.0 °C Show Material materials with Melting point of 1540.0 - 1715.0 °C | Typical for Titanium Alpha Alloy |
Specific heat capacity | 460.0 - 527.0 J/(kg·K) Show Material materials with Specific heat capacity of 460.0 - 527.0 J/(kg·K) | Typical for Titanium Alpha Alloy |
Thermal conductivity | 4.0 - 17.0 W/(m·K) Show Material materials with Thermal conductivity of 4.0 - 17.0 W/(m·K) | Typical for Titanium Alpha Alloy |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.1 Show Material materials with Carbon of 0.1 | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Copper | 2.0 - 3.0 % Show Material materials with Copper of 2.0 - 3.0 % | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Hydrogen | 0.01 Show Material materials with Hydrogen of 0.01 | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Iron | 0.2 Show Material materials with Iron of 0.2 | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Nitrogen | 0.05 Show Material materials with Nitrogen of 0.05 | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Oxygen | 0.2 Show Material materials with Oxygen of 0.2 | Annealed | WL 3.7124-1 | Forging, Rod, Flat |
Titanium | 96.4 % Show Material materials with Titanium of 96.4 % | Annealed | WL 3.7124-1 | Forging, Rod, Flat |