General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 5 g/cm³ Show Material materials with Density of 5 g/cm³ | Typical for Zinc Aluminium |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation A10 | 20.0 °C | 60 - 80 % Show Material materials with Elongation A10 of 60 - 80 % | |
Hardness, Brinell | 20.0 °C | 40 - 50 [-] Show Material materials with Hardness, Brinell of 40 - 50 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Zinc Aluminium |
Tensile strength | 20.0 °C | 200 - 240 MPa Show Material materials with Tensile strength of 200 - 240 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.2E-5 - 2.8E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.8E-5 1/K | Typical for Zinc Aluminium |
Melting point | 375 - 485 °C Show Material materials with Melting point of 375 - 485 °C | Typical for Zinc Aluminium | |
Specific heat capacity | 23.0 °C | 393 - 525 J/(kg·K) Show Material materials with Specific heat capacity of 393 - 525 J/(kg·K) | Typical for Zinc Aluminium |
Thermal conductivity | 23.0 °C | 105 - 125 W/(m·K) Show Material materials with Thermal conductivity of 105 - 125 W/(m·K) | Typical for Zinc Aluminium |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.7 - 0.9 % Show Material materials with Aluminium of 0.7 - 0.9 % |
Copper | 0.3 - 0.5 % Show Material materials with Copper of 0.3 - 0.5 % |
Zinc | 98.6 % Show Material materials with Zinc of 98.6 % |