Zinkberatung e. V. 1981 Grade G-ZnAl27Cu2 cast condition

Want to keep this datasheet? Save it now in your required format

Description

The material ZnAl27Cu2, a fine zinc block metal alloy acc. to ASTM B 669, german marking ZA 27, is used with the transition coming from malleable cast iron or cast iron with nodular graphite, brass or bronze, where it depends on highest strength and strain. ZA 27 is the best alloy for operatings temperature to 120 °C. The alloy is pressure tight, even in thin cross sections. Where however highest pressure tight ones is necessary, the alloys ZnAl8 or ZnAl12 should be considered. The material is excellently machinable and on high polish sharpening and polishingable. The alloy is used mainly for sand and ingot casting, in addition, for pressure casting on cold chamber machines.

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

5 g/cm³

Show Material materials with Density of 5 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

75 GPa

Show Material materials with Elastic modulus of 75 GPa

Elongation A50

20.0 °C

3 - 6 %

Show Material materials with Elongation A50 of 3 - 6 %

Hardness, Brinell

20.0 °C

110 - 120 [-]

Show Material materials with Hardness, Brinell of 110 - 120 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Zinc Aluminium

Tensile strength

20.0 °C

400 - 440 MPa

Show Material materials with Tensile strength of 400 - 440 MPa

Yield strength Rp0.2

20.0 °C

338 - 345 MPa

Show Material materials with Yield strength Rp0.2 of 338 - 345 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.2E-5 - 2.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.2E-5 - 2.8E-5 1/K

Typical for Zinc Aluminium

Melting point

375 - 485 °C

Show Material materials with Melting point of 375 - 485 °C

Typical for Zinc Aluminium

Specific heat capacity

23.0 °C

393 - 525 J/(kg·K)

Show Material materials with Specific heat capacity of 393 - 525 J/(kg·K)

Typical for Zinc Aluminium

Thermal conductivity

23.0 °C

105 - 125 W/(m·K)

Show Material materials with Thermal conductivity of 105 - 125 W/(m·K)

Typical for Zinc Aluminium

Chemical properties

PropertyValue

Aluminium

25 - 28 %

Show Material materials with Aluminium of 25 - 28 %

Cadmium

3E-3 %

Show Material materials with Cadmium of 3E-3 %

Copper

2 - 2.5 %

Show Material materials with Copper of 2 - 2.5 %

Iron

0.1 %

Show Material materials with Iron of 0.1 %

Lead

4E-3 %

Show Material materials with Lead of 4E-3 %

Magnesium

0.01 - 0.02 %

Show Material materials with Magnesium of 0.01 - 0.02 %

Tin

2E-3 %

Show Material materials with Tin of 2E-3 %

Zinc

69.37 %

Show Material materials with Zinc of 69.37 %

Technological properties

Property
Processing methods

sand casting