General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 12.16 g/cm³ Show Material materials with Density of 12.16 g/cm³ | Typical for Palladium |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -195.0 °C | 126 GPa Show Material materials with Elastic modulus of 126 GPa | |
20.0 °C | 124 GPa Show Material materials with Elastic modulus of 124 GPa | ||
250.0 °C | 121 GPa Show Material materials with Elastic modulus of 121 GPa | ||
400.0 °C | 119 GPa Show Material materials with Elastic modulus of 119 GPa | ||
500.0 °C | 117 GPa Show Material materials with Elastic modulus of 117 GPa | ||
600.0 °C | 113 GPa Show Material materials with Elastic modulus of 113 GPa | ||
750.0 °C | 98 GPa Show Material materials with Elastic modulus of 98 GPa | ||
800.0 °C | 91 GPa Show Material materials with Elastic modulus of 91 GPa | ||
Hardness, Vickers | 20.0 °C | 90 [-] Show Material materials with Hardness, Vickers of 90 [-] | |
Poisson's ratio | 23.0 °C | 0.39 [-] Show Material materials with Poisson's ratio of 0.39 [-] | Typical for Palladium |
Shear modulus | 23.0 °C | 42 GPa Show Material materials with Shear modulus of 42 GPa | Typical for Palladium |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 50.0 °C | 1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K | |
100.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | ||
200.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
300.0 °C | 1.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.23E-5 1/K | ||
400.0 °C | 1.26E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.26E-5 1/K | ||
500.0 °C | 1.28E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.28E-5 1/K | ||
600.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | ||
700.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
800.0 °C | 1.34E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.34E-5 1/K | ||
900.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | ||
1000.0 °C | 1.39E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.39E-5 1/K | ||
Melting point | 1553 °C Show Material materials with Melting point of 1553 °C | Typical for Palladium | |
Specific heat capacity | 23.0 °C | 236 - 248 J/(kg·K) Show Material materials with Specific heat capacity of 236 - 248 J/(kg·K) | Typical for Palladium |
Thermal conductivity | -173.0 °C | 76 W/(m·K) Show Material materials with Thermal conductivity of 76 W/(m·K) | |
-73.0 °C | 75 W/(m·K) Show Material materials with Thermal conductivity of 75 W/(m·K) | ||
127.0 °C | 75.5 W/(m·K) Show Material materials with Thermal conductivity of 75.5 W/(m·K) | ||
327.0 °C | 79 W/(m·K) Show Material materials with Thermal conductivity of 79 W/(m·K) | ||
527.0 °C | 83 W/(m·K) Show Material materials with Thermal conductivity of 83 W/(m·K) | ||
727.0 °C | 87 W/(m·K) Show Material materials with Thermal conductivity of 87 W/(m·K) | ||
927.0 °C | 88.2 W/(m·K) Show Material materials with Thermal conductivity of 88.2 W/(m·K) | ||
1127.0 °C | 86.9 W/(m·K) Show Material materials with Thermal conductivity of 86.9 W/(m·K) | ||
1327.0 °C | 86 W/(m·K) Show Material materials with Thermal conductivity of 86 W/(m·K) | ||
Chemical properties
Property | Value |
---|---|
Palladium | 99.9 % Show Material materials with Palladium of 99.9 % |