General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 21.5 g/cm³ Show Material materials with Density of 21.5 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -195.0 °C | 178 GPa Show Material materials with Elastic modulus of 178 GPa |
20.0 °C | 170 - 173 GPa Show Material materials with Elastic modulus of 170 - 173 GPa | |
250.0 °C | 169 GPa Show Material materials with Elastic modulus of 169 GPa | |
400.0 °C | 163 GPa Show Material materials with Elastic modulus of 163 GPa | |
500.0 °C | 159 GPa Show Material materials with Elastic modulus of 159 GPa | |
600.0 °C | 153 GPa Show Material materials with Elastic modulus of 153 GPa | |
750.0 °C | 140 GPa Show Material materials with Elastic modulus of 140 GPa | |
800.0 °C | 136 GPa Show Material materials with Elastic modulus of 136 GPa | |
900.0 °C | 126 GPa Show Material materials with Elastic modulus of 126 GPa | |
1000.0 °C | 115 GPa Show Material materials with Elastic modulus of 115 GPa | |
Hardness, Vickers | 20.0 °C | 100 [-] Show Material materials with Hardness, Vickers of 100 [-] |
Poisson's ratio | 20.0 °C | 0.39 [-] Show Material materials with Poisson's ratio of 0.39 [-] |
Shear modulus | 20.0 °C | 67 GPa Show Material materials with Shear modulus of 67 GPa |
Tensile strength | 20.0 °C | 200 - 300 MPa Show Material materials with Tensile strength of 200 - 300 MPa |
Yield strength | 20.0 °C | 185 MPa Show Material materials with Yield strength of 185 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 9.1E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.1E-6 1/K | |
200.0 °C | 9.2E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.2E-6 1/K | ||
300.0 °C | 9.3E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.3E-6 1/K | ||
400.0 °C | 9.5E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.5E-6 1/K | ||
500.0 °C | 9.6E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.6E-6 1/K | ||
600.0 °C | 9.7E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.7E-6 1/K | ||
700.0 °C | 9.9E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K | ||
800.0 °C | 1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1E-5 1/K | ||
900.0 °C | 1.01E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.01E-5 1/K | ||
1000.0 °C | 1.03E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.03E-5 1/K | ||
1100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | ||
1200.0 °C | 1.06E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.06E-5 1/K | ||
1300.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | ||
1400.0 °C | 1.1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K | ||
1500.0 °C | 1.12E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.12E-5 1/K | ||
1600.0 °C | 1.14E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.14E-5 1/K | ||
Melting point | 1769 °C Show Material materials with Melting point of 1769 °C | Typical for Platinum | |
Specific heat capacity | 23.0 °C | 136 J/(kg·K) Show Material materials with Specific heat capacity of 136 J/(kg·K) | Typical for Platinum |
Thermal conductivity | -173.0 °C | 85.6 W/(m·K) Show Material materials with Thermal conductivity of 85.6 W/(m·K) | |
-73.0 °C | 79 W/(m·K) Show Material materials with Thermal conductivity of 79 W/(m·K) | ||
20.0 °C | 74 W/(m·K) Show Material materials with Thermal conductivity of 74 W/(m·K) | ||
127.0 °C | 73.2 W/(m·K) Show Material materials with Thermal conductivity of 73.2 W/(m·K) | ||
327.0 °C | 73 W/(m·K) Show Material materials with Thermal conductivity of 73 W/(m·K) | ||
527.0 °C | 74.8 W/(m·K) Show Material materials with Thermal conductivity of 74.8 W/(m·K) | ||
727.0 °C | 76.9 W/(m·K) Show Material materials with Thermal conductivity of 76.9 W/(m·K) | ||
927.0 °C | 83.2 W/(m·K) Show Material materials with Thermal conductivity of 83.2 W/(m·K) | ||
1127.0 °C | 88.3 W/(m·K) Show Material materials with Thermal conductivity of 88.3 W/(m·K) | ||
1327.0 °C | 89.5 W/(m·K) Show Material materials with Thermal conductivity of 89.5 W/(m·K) | ||
1527.0 °C | 89 W/(m·K) Show Material materials with Thermal conductivity of 89 W/(m·K) | ||
1727.0 °C | 86 W/(m·K) Show Material materials with Thermal conductivity of 86 W/(m·K) | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 20.0 °C | 9.40E+6 S/m Show Material materials with Electrical conductivity of 9.40E+6 S/m |
Electrical resistivity | 20.0 °C | 1.16E-7 Ω·m Show Material materials with Electrical resistivity of 1.16E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Platinum | 99.5 - 99.99 % Show Material materials with Platinum of 99.5 - 99.99 % |