General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 19.2 g/cm³ Show Material materials with Density of 19.2 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | |
Elongation | 20.0 °C | 2 % Show Material materials with Elongation of 2 % | |
Hardness, Vickers | 20.0 °C | 360 [-] Show Material materials with Hardness, Vickers of 360 [-] | |
Poisson's ratio | 23.0 °C | 0.39 [-] Show Material materials with Poisson's ratio of 0.39 [-] | Typical for Platinum |
Shear modulus | 20.0 °C | 73 GPa Show Material materials with Shear modulus of 73 GPa | |
Tensile strength | 20.0 °C | 1270 MPa Show Material materials with Tensile strength of 1270 MPa | |
Yield strength Rp0.2 | 20.0 °C | 920 MPa Show Material materials with Yield strength Rp0.2 of 920 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 300.0 °C | 1.04E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 1/K | |
Melting point | 1769 °C Show Material materials with Melting point of 1769 °C | Typical for Platinum | |
Specific heat capacity | 23.0 °C | 136 J/(kg·K) Show Material materials with Specific heat capacity of 136 J/(kg·K) | Typical for Platinum |
Thermal conductivity | 23.0 °C | 69 - 73 W/(m·K) Show Material materials with Thermal conductivity of 69 - 73 W/(m·K) | Typical for Platinum |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.79E-7 Ω·m Show Material materials with Electrical resistivity of 2.79E-7 Ω·m |