Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.65 - 7.7 g/cm³ Show Material materials with Dichte of 7.65 - 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 7 - 20 % Show Material materials with Dehnung of 7 - 20 % | |
Elastizitätsmodul | 20.0 °C | 196 - 220 GPa Show Material materials with Elastizitätsmodul of 196 - 220 GPa | |
100.0 °C | 215 GPa Show Material materials with Elastizitätsmodul of 215 GPa | ||
200.0 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | ||
300.0 °C | 205 GPa Show Material materials with Elastizitätsmodul of 205 GPa | ||
400.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | ||
Hardness, Brinell, trans | 20.0 °C | 200 [-] Show Material materials with Hardness, Brinell, trans of 200 [-] | |
Härte, Brinell | 20.0 °C | 200 [-] Show Material materials with Härte, Brinell of 200 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Martensitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Martensitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 250 - 330 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 - 330 MPa | |
100.0 °C | 230 MPa Show Material materials with Streckgrenze Rp 0,2 of 230 MPa | ||
150.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2 of 220 MPa | ||
200.0 °C | 215 MPa Show Material materials with Streckgrenze Rp 0,2 of 215 MPa | ||
250.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 0,2 of 210 MPa | ||
300.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2 of 205 MPa | ||
350.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | ||
400.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 0,2 of 195 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 250 MPa | |
Zugfestigkeit | 20.0 °C | 430 - 950 MPa Show Material materials with Zugfestigkeit of 430 - 950 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 430 - 630 MPa Show Material materials with Zugfestigkeit, transversal of 430 - 630 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 9.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.2E-6 1/K | |
20.0 °C | 9.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.9E-6 1/K | ||
100.0 °C | 1E-5 - 1.03E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.03E-5 1/K | ||
200.0 °C | 1.05E-5 - 1.08E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.08E-5 1/K | ||
300.0 °C | 1.05E-5 - 1.12E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.05E-5 - 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.1E-5 - 1.19E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29E-5 1/K | ||
900.0 °C | 1.34E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34E-5 1/K | ||
1000.0 °C | 1.39E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.39E-5 1/K | ||
Schmelzpunkt | 1370 - 1530 °C Show Material materials with Schmelzpunkt of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 450 - 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 616 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | |
Wärmeleitfähigkeit | 20.0 °C | 19.6 - 25 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 19.6 - 25 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 6.17E-7 - 7E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.17E-7 - 7E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 16 - 18 % Show Material materials with Chrom of 16 - 18 % |
Kohlenstoff | 0.08 % Show Material materials with Kohlenstoff of 0.08 % |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % |
Molybdän | 0.2 - 0.6 % Show Material materials with Molybdän of 0.2 - 0.6 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.15 - 0.35 % Show Material materials with Schwefel of 0.15 - 0.35 % |
Silizium | 1.5 % Show Material materials with Silizium of 1.5 % |