Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 20.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 37 % Show Material materials with Dehnung of 37 % | |
Dehnung A50 | 20.0 °C | 28 - 36 % Show Material materials with Dehnung A50 of 28 - 36 % | |
Dehnung A80 | 20.0 °C | 26 - 34 % Show Material materials with Dehnung A80 of 26 - 34 % | |
Elastizitätsmodul | 20.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel |
Härte, Vickers | 20.0 °C | 110 - 120 [-] Show Material materials with Härte, Vickers of 110 - 120 [-] | |
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel |
Streckgrenze | 20.0 °C | 140 - 280 MPa Show Material materials with Streckgrenze of 140 - 280 MPa | |
Zugfestigkeit | 20.0 °C | 270 - 370 MPa Show Material materials with Zugfestigkeit of 270 - 370 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.32E-5 - 1.38E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 - 1.38E-5 1/K | Typical for Low Carbon Steel |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties