Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.1 g/cm³ Show Material materials with Dichte of 8.1 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 25 % Show Material materials with Dehnung of 25 % | |
Elastizitätsmodul | 20.0 °C | 215 GPa Show Material materials with Elastizitätsmodul of 215 GPa | |
Flächenreduzierung | 20.0 °C | 30 % Show Material materials with Flächenreduzierung of 30 % | |
Härte, Rockwell C | 20.0 °C | 28 [-] Show Material materials with Härte, Rockwell C of 28 [-] | |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Nickel Steel |
Schubmodule | 23.0 °C | 76 GPa Show Material materials with Schubmodule of 76 GPa | Typical for Nickel Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 500 MPa Show Material materials with Streckgrenze Rp 0,2 of 500 MPa | |
500.0 °C | 450 MPa Show Material materials with Streckgrenze Rp 0,2 of 450 MPa | ||
550.0 °C | 450 MPa Show Material materials with Streckgrenze Rp 0,2 of 450 MPa | ||
600.0 °C | 450 MPa Show Material materials with Streckgrenze Rp 0,2 of 450 MPa | ||
650.0 °C | 430 MPa Show Material materials with Streckgrenze Rp 0,2 of 430 MPa | ||
700.0 °C | 430 MPa Show Material materials with Streckgrenze Rp 0,2 of 430 MPa | ||
750.0 °C | 380 MPa Show Material materials with Streckgrenze Rp 0,2 of 380 MPa | ||
800.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 MPa | ||
Zugfestigkeit | 20.0 °C | 900 - 1100 MPa Show Material materials with Zugfestigkeit of 900 - 1100 MPa | |
500.0 °C | 800 MPa Show Material materials with Zugfestigkeit of 800 MPa | ||
550.0 °C | 800 MPa Show Material materials with Zugfestigkeit of 800 MPa | ||
600.0 °C | 790 MPa Show Material materials with Zugfestigkeit of 790 MPa | ||
650.0 °C | 740 MPa Show Material materials with Zugfestigkeit of 740 MPa | ||
700.0 °C | 640 MPa Show Material materials with Zugfestigkeit of 640 MPa | ||
750.0 °C | 500 MPa Show Material materials with Zugfestigkeit of 500 MPa | ||
800.0 °C | 340 MPa Show Material materials with Zugfestigkeit of 340 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.41E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41E-5 1/K | |
300.0 °C | 1.55E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.55E-5 1/K | ||
500.0 °C | 1.59E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.59E-5 1/K | ||
700.0 °C | 1.68E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.68E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 700 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 700 °C | ||
Schmelzpunkt | 1316 - 1595 °C Show Material materials with Schmelzpunkt of 1316 - 1595 °C | Typical for Nickel Steel | |
Spezifische Wärmekapazität | 20.0 °C | 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 13 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 13 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.3 - 1 % Show Material materials with Aluminium of 0.3 - 1 % |
Bor | 8E-3 % Show Material materials with Bor of 8E-3 % |
Chrom | 18 - 21 % Show Material materials with Chrom of 18 - 21 % |
Eisen | 23 - 28 % Show Material materials with Eisen of 23 - 28 % |
Kohlenstoff | 0.1 % Show Material materials with Kohlenstoff of 0.1 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Titan | 1 - 2 % Show Material materials with Titan of 1 - 2 % |