Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.3 % Show Material materials with Dehnung of 18.3 % | Predicted Value, A80 Transverse | ||||
18.6 % Show Material materials with Dehnung of 18.6 % | Predicted Value, A200 | |||||
21.1 % Show Material materials with Dehnung of 21.1 % | Predicted Value, A5 | |||||
23.3 % Show Material materials with Dehnung of 23.3 % | Predicted Value, A50 | |||||
23.9 % Show Material materials with Dehnung of 23.9 % | Predicted Value, Transverse | |||||
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized or normalized formed (+N) | EN 10149-3 | Flat | A80 | |
20 °C | 30 % Show Material materials with Dehnung of 30 % | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Flächenreduzierung | 40.6 % Show Material materials with Flächenreduzierung of 40.6 % | Predicted Value | ||||
44.1 % Show Material materials with Flächenreduzierung of 44.1 % | Predicted Value, Transverse | |||||
Härte, Brinell | 241 [-] Show Material materials with Härte, Brinell of 241 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 498.4 MPa Show Material materials with Scherfestigkeit of 498.4 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 247.6 MPa Show Material materials with Streckgrenze of 247.6 MPa | Predicted Value, RP1 | ||||
299.1 MPa Show Material materials with Streckgrenze of 299.1 MPa | Predicted Value, RP1 Transverse | |||||
301.7 MPa Show Material materials with Streckgrenze of 301.7 MPa | Predicted Value, RP02 | |||||
322 MPa Show Material materials with Streckgrenze of 322 MPa | Predicted Value, Transverse | |||||
398.4 MPa Show Material materials with Streckgrenze of 398.4 MPa | Predicted Value, RP05 | |||||
467.6 MPa Show Material materials with Streckgrenze of 467.6 MPa | Predicted Value, RP02 Transverse | |||||
483.4 MPa Show Material materials with Streckgrenze of 483.4 MPa | Predicted Value, RP002 | |||||
20 °C | 260 MPa Show Material materials with Streckgrenze of 260 MPa | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Zugfestigkeit | 20 °C | 370 - 490 MPa Show Material materials with Zugfestigkeit of 370 - 490 MPa | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Max. Betriebstemperatur | -20 °C Show Material materials with Max. Betriebstemperatur of -20 °C | normalized or normalized formed (+N) | EN 10149-3 | Flat | Long | |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Temperaturleitfähigkeit | -100 °C | 18 mm²/s Show Material materials with Temperaturleitfähigkeit of 18 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 14.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 14.8 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 13.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 13.7 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 12.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 10.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.6 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 7.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.6 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 6.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.1 mm²/s | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
Wärmeleitfähigkeit | -100 °C | 52.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 52.6 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 53.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 53.4 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 53.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 53.3 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 50.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50.1 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 46.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.9 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 43.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 39.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.5 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 36.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.1 W/(m·K) | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value | ||||
spezifischer Widerstand | -100 °C | 1.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | |
20 °C | 1.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
100 °C | 2.4e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.4e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
200 °C | 3.15e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.15e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
300 °C | 4e-07 Ω·m Show Material materials with spezifischer Widerstand of 4e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
400 °C | 5.03e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.03e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
500 °C | 6.26e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.26e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat | ||
600 °C | 7.68e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Kohlenstoff | 0.16 % Show Material materials with Kohlenstoff of 0.16 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Mangan | 1.2 % Show Material materials with Mangan of 1.2 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Niobium | 0.09 % Show Material materials with Niobium of 0.09 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Schwefel | 0.02 % Show Material materials with Schwefel of 0.02 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |
Vanadium | 0.1 % Show Material materials with Vanadium of 0.1 % | normalized or normalized formed (+N) | EN 10149-3 | Flat |