Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized and tempered (+NT) | EN 10028-4 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.6 % Show Material materials with Dehnung of 18.6 % | Predicted Value, A200 | ||||
18.9 % Show Material materials with Dehnung of 18.9 % | Predicted Value, A80 Transverse | |||||
19.6 % Show Material materials with Dehnung of 19.6 % | Predicted Value, A80 | |||||
21.3 % Show Material materials with Dehnung of 21.3 % | Predicted Value, A5 | |||||
21.7 % Show Material materials with Dehnung of 21.7 % | Predicted Value, A50 | |||||
21.8 % Show Material materials with Dehnung of 21.8 % | Predicted Value, Transverse | |||||
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Flächenreduzierung | 39.8 % Show Material materials with Flächenreduzierung of 39.8 % | Predicted Value | ||||
44.1 % Show Material materials with Flächenreduzierung of 44.1 % | Predicted Value, Transverse | |||||
Poissonzahl | 0.291 [-] Show Material materials with Poissonzahl of 0.291 [-] | Typical for Nickel Steel | ||||
Scherfestigkeit | 532.4 MPa Show Material materials with Scherfestigkeit of 532.4 MPa | Predicted Value | ||||
Schubmodule | 76 GPa Show Material materials with Schubmodule of 76 GPa | Typical for Nickel Steel | ||||
Streckgrenze | 257.4 MPa Show Material materials with Streckgrenze of 257.4 MPa | Predicted Value, RP1 | ||||
300.2 MPa Show Material materials with Streckgrenze of 300.2 MPa | Predicted Value, RP1 Transverse | |||||
329 MPa Show Material materials with Streckgrenze of 329 MPa | Predicted Value, RP02 | |||||
342.8 MPa Show Material materials with Streckgrenze of 342.8 MPa | Predicted Value, Transverse | |||||
380.6 MPa Show Material materials with Streckgrenze of 380.6 MPa | Predicted Value, RP05 | |||||
463.6 MPa Show Material materials with Streckgrenze of 463.6 MPa | Predicted Value, RP02 Transverse | |||||
463.8 MPa Show Material materials with Streckgrenze of 463.8 MPa | Predicted Value, RP002 | |||||
20 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
20 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Zugfestigkeit | 20 °C | 420 - 530 MPa Show Material materials with Zugfestigkeit of 420 - 530 MPa | normalized and tempered (+NT) | EN 10028-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Schmelzpunkt | 1316 - 1595 °C Show Material materials with Schmelzpunkt of 1316 - 1595 °C | Typical for Nickel Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 11.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 11.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.2 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 9.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 7 mm²/s Show Material materials with Temperaturleitfähigkeit of 7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
Wärmeleitfähigkeit | 20 °C | 42.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 43.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 42.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.8 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 40.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 36.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.4 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.1 W/(m·K) | normalized and tempered (+NT) | EN 10028-4 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 6 S/m Show Material materials with Elektrische Leitfähigkeit of 6 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.45e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.45e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | |
100 °C | 2.94e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
200 °C | 3.69e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.69e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
300 °C | 4.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.59e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
400 °C | 5.58e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.58e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
500 °C | 6.79e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.79e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.13e-07 Ω·m | normalized and tempered (+NT) | EN 10028-4 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Kohlenstoff | 0.14 % Show Material materials with Kohlenstoff of 0.14 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Mangan | 0.7 - 1.5 % Show Material materials with Mangan of 0.7 - 1.5 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Nickel | 0.3 - 0.8 % Show Material materials with Nickel of 0.3 - 0.8 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
0.015 % Show Material materials with Schwefel of 0.015 % | normalized and tempered (+NT) | EN 10028-4 | Flat | |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized and tempered (+NT) | EN 10028-4 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |