Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.4 % Show Material materials with Dehnung of 18.4 % | Predicted Value, A200 | ||||
22.1 % Show Material materials with Dehnung of 22.1 % | Predicted Value, A5 | |||||
24.4 % Show Material materials with Dehnung of 24.4 % | Predicted Value, A50 | |||||
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Dehnung of 23 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 25 % Show Material materials with Dehnung of 25 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 26 % Show Material materials with Dehnung of 26 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Poissonzahl | 20 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Streckgrenze | 249.4 MPa Show Material materials with Streckgrenze of 249.4 MPa | Predicted Value, RP1 | ||||
278.8 MPa Show Material materials with Streckgrenze of 278.8 MPa | Predicted Value, RP1 Transverse | |||||
288.4 MPa Show Material materials with Streckgrenze of 288.4 MPa | Predicted Value, RP05 | |||||
318.4 MPa Show Material materials with Streckgrenze of 318.4 MPa | Predicted Value, RP02 | |||||
346.3 MPa Show Material materials with Streckgrenze of 346.3 MPa | Predicted Value, RP02 Transverse | |||||
467 MPa Show Material materials with Streckgrenze of 467 MPa | Predicted Value, RP002 | |||||
20 °C | 195 MPa Show Material materials with Streckgrenze of 195 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 195 MPa Show Material materials with Streckgrenze of 195 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Zugfestigkeit | 20 °C | 340 - 510 MPa Show Material materials with Zugfestigkeit of 340 - 510 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
20 °C | 340 - 470 MPa Show Material materials with Zugfestigkeit of 340 - 470 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 350 - 510 MPa Show Material materials with Zugfestigkeit of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 350 - 500 MPa Show Material materials with Zugfestigkeit of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 350 - 510 MPa Show Material materials with Zugfestigkeit of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 500 MPa Show Material materials with Zugfestigkeit of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Zugfestigkeit of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 360 - 500 MPa Show Material materials with Zugfestigkeit of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 360 - 510 MPa Show Material materials with Zugfestigkeit of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 360 - 500 MPa Show Material materials with Zugfestigkeit of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 470 MPa Show Material materials with Zugfestigkeit of 360 - 470 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Temperaturleitfähigkeit | 20 °C | 15.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 15.7 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 14.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 14.5 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 12.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 11.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 9.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.6 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 7.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.9 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 6.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.3 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Wärmeleitfähigkeit | 20 °C | 56.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 56.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 56.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 56.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 53.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 53.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 49.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 49.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 45.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 41.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 37.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | 20 °C | 1.83e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.83e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 2.27e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 2.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 3.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 4.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.81e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 5.99e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.99e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 7.38e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.38e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.4 - 0.8 % Show Material materials with Chrom of 0.4 - 0.8 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kohlenstoff | 0.13 % Show Material materials with Kohlenstoff of 0.13 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kupfer | 0.25 - 0.55 % Show Material materials with Kupfer of 0.25 - 0.55 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mangan | 0.2 - 0.8 % Show Material materials with Mangan of 0.2 - 0.8 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nickel | 0.65 % Show Material materials with Nickel of 0.65 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Phosphor | 0.035 % Show Material materials with Phosphor of 0.035 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.04 % Show Material materials with Phosphor of 0.04 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.035 % Show Material materials with Schwefel of 0.035 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |