Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 17.5 % Show Material materials with Dehnung of 17.5 % | Predicted Value, A200 | ||||
22.6 % Show Material materials with Dehnung of 22.6 % | Predicted Value, A5 | |||||
23.1 % Show Material materials with Dehnung of 23.1 % | Predicted Value, A50 | |||||
20 °C | 14 % Show Material materials with Dehnung of 14 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 15 % Show Material materials with Dehnung of 15 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | ||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Streckgrenze | 261.8 MPa Show Material materials with Streckgrenze of 261.8 MPa | Predicted Value, RP1 | ||||
285.8 MPa Show Material materials with Streckgrenze of 285.8 MPa | Predicted Value, RP1 Transverse | |||||
370.2 MPa Show Material materials with Streckgrenze of 370.2 MPa | Predicted Value, RP05 | |||||
392.1 MPa Show Material materials with Streckgrenze of 392.1 MPa | Predicted Value, RP02 | |||||
400.2 MPa Show Material materials with Streckgrenze of 400.2 MPa | Predicted Value, RP02 Transverse | |||||
497.1 MPa Show Material materials with Streckgrenze of 497.1 MPa | Predicted Value, RP002 | |||||
20 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Zugfestigkeit | 20 °C | 470 - 680 MPa Show Material materials with Zugfestigkeit of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse |
20 °C | 470 - 630 MPa Show Material materials with Zugfestigkeit of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 470 - 680 MPa Show Material materials with Zugfestigkeit of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 630 MPa Show Material materials with Zugfestigkeit of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 490 - 680 MPa Show Material materials with Zugfestigkeit of 490 - 680 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Zugfestigkeit of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 510 - 680 MPa Show Material materials with Zugfestigkeit of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 510 - 630 MPa Show Material materials with Zugfestigkeit of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 510 - 680 MPa Show Material materials with Zugfestigkeit of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 510 - 630 MPa Show Material materials with Zugfestigkeit of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 - 1.25 % Show Material materials with Chrom of 0.3 - 1.25 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kohlenstoff | 0.12 % Show Material materials with Kohlenstoff of 0.12 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kupfer | 0.25 - 0.55 % Show Material materials with Kupfer of 0.25 - 0.55 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mangan | 1 % Show Material materials with Mangan of 1 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nickel | 0.65 % Show Material materials with Nickel of 0.65 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Phosphor | 0.06 - 0.15 % Show Material materials with Phosphor of 0.06 - 0.15 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.04 % Show Material materials with Schwefel of 0.04 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Silizium | 0.75 % Show Material materials with Silizium of 0.75 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Stickstoff | 0.009 % Show Material materials with Stickstoff of 0.009 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |