Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.5 % Show Material materials with Dehnung of 18.5 % | Predicted Value, A200 | ||||
20.8 % Show Material materials with Dehnung of 20.8 % | Predicted Value, A5 | |||||
21.0 % Show Material materials with Dehnung of 21.0 % | Predicted Value, A80 Transverse | |||||
23.9 % Show Material materials with Dehnung of 23.9 % | Predicted Value, Transverse | |||||
25.6 % Show Material materials with Dehnung of 25.6 % | Predicted Value, A50 | |||||
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | A80 | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | A80 | |
20 °C | 25 % Show Material materials with Dehnung of 25 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | ||
20 °C | 26 % Show Material materials with Dehnung of 26 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | ||
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Flächenreduzierung | 43.7 % Show Material materials with Flächenreduzierung of 43.7 % | Predicted Value, Transverse | ||||
44.0 % Show Material materials with Flächenreduzierung of 44.0 % | Predicted Value | |||||
Härte, Brinell | 242 [-] Show Material materials with Härte, Brinell of 242 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 525.6 MPa Show Material materials with Scherfestigkeit of 525.6 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 252.2 MPa Show Material materials with Streckgrenze of 252.2 MPa | Predicted Value, RP1 | ||||
282.7 MPa Show Material materials with Streckgrenze of 282.7 MPa | Predicted Value, RP05 | |||||
297.5 MPa Show Material materials with Streckgrenze of 297.5 MPa | Predicted Value, Transverse | |||||
315.9 MPa Show Material materials with Streckgrenze of 315.9 MPa | Predicted Value, RP1 Transverse | |||||
455.8 MPa Show Material materials with Streckgrenze of 455.8 MPa | Predicted Value, RP002 | |||||
472.6 MPa Show Material materials with Streckgrenze of 472.6 MPa | Predicted Value, RP02 Transverse | |||||
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | ||
20 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | ||
20 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | ||
100 °C | 171 MPa Show Material materials with Streckgrenze of 171 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | RP02 | |
150 °C | 162 MPa Show Material materials with Streckgrenze of 162 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | RP02 | |
200 °C | 153 MPa Show Material materials with Streckgrenze of 153 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | RP02 | |
250 °C | 135 MPa Show Material materials with Streckgrenze of 135 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | RP02 | |
300 °C | 117 MPa Show Material materials with Streckgrenze of 117 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar | RP02 | |
Zugfestigkeit | 20 °C | 360 - 480 MPa Show Material materials with Zugfestigkeit of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 319.3 °C Show Material materials with Max. Betriebstemperatur of 319.3 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Kohlenstoff | 0.16 % Show Material materials with Kohlenstoff of 0.16 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Mangan | 0.4 - 1.2 % Show Material materials with Mangan of 0.4 - 1.2 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | normalized or normalized formed (+N) | EN 10207 | Strip, Sheet, Bar |