Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 40 % Show Material materials with Dehnung of 40 % | |
Dehnung, transversal | 20.0 °C | 30 % Show Material materials with Dehnung, transversal of 30 % | |
Elastizitätsmodul | 20.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Elastizitätsmodul of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
Hardness, Brinell, trans | 20.0 °C | 215 [-] Show Material materials with Hardness, Brinell, trans of 215 [-] | |
Härte, Brinell | 20.0 °C | 215 [-] Show Material materials with Härte, Brinell of 215 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | |
100.0 °C | 165 MPa Show Material materials with Streckgrenze Rp 0,2 of 165 MPa | ||
150.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 MPa | ||
200.0 °C | 137 MPa Show Material materials with Streckgrenze Rp 0,2 of 137 MPa | ||
250.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 0,2 of 127 MPa | ||
300.0 °C | 119 MPa Show Material materials with Streckgrenze Rp 0,2 of 119 MPa | ||
350.0 °C | 113 MPa Show Material materials with Streckgrenze Rp 0,2 of 113 MPa | ||
400.0 °C | 108 MPa Show Material materials with Streckgrenze Rp 0,2 of 108 MPa | ||
450.0 °C | 103 MPa Show Material materials with Streckgrenze Rp 0,2 of 103 MPa | ||
500.0 °C | 100 MPa Show Material materials with Streckgrenze Rp 0,2 of 100 MPa | ||
550.0 °C | 98 MPa Show Material materials with Streckgrenze Rp 0,2 of 98 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 200 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 235 MPa Show Material materials with Streckgrenze Rp 1,0 of 235 MPa | |
100.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 1,0 of 200 MPa | ||
150.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 1,0 of 180 MPa | ||
200.0 °C | 165 MPa Show Material materials with Streckgrenze Rp 1,0 of 165 MPa | ||
250.0 °C | 153 MPa Show Material materials with Streckgrenze Rp 1,0 of 153 MPa | ||
300.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 1,0 of 145 MPa | ||
350.0 °C | 139 MPa Show Material materials with Streckgrenze Rp 1,0 of 139 MPa | ||
400.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 1,0 of 135 MPa | ||
450.0 °C | 130 MPa Show Material materials with Streckgrenze Rp 1,0 of 130 MPa | ||
500.0 °C | 128 MPa Show Material materials with Streckgrenze Rp 1,0 of 128 MPa | ||
550.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 1,0 of 127 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 235 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 235 MPa | |
Zugfestigkeit | 20.0 °C | 500 - 700 MPa Show Material materials with Zugfestigkeit of 500 - 700 MPa | |
100.0 °C | 430 MPa Show Material materials with Zugfestigkeit of 430 MPa | ||
150.0 °C | 410 MPa Show Material materials with Zugfestigkeit of 410 MPa | ||
200.0 °C | 390 MPa Show Material materials with Zugfestigkeit of 390 MPa | ||
250.0 °C | 385 MPa Show Material materials with Zugfestigkeit of 385 MPa | ||
300.0 °C | 380 MPa Show Material materials with Zugfestigkeit of 380 MPa | ||
350.0 °C | 380 MPa Show Material materials with Zugfestigkeit of 380 MPa | ||
400.0 °C | 380 MPa Show Material materials with Zugfestigkeit of 380 MPa | ||
450.0 °C | 375 MPa Show Material materials with Zugfestigkeit of 375 MPa | ||
500.0 °C | 360 MPa Show Material materials with Zugfestigkeit of 360 MPa | ||
Zugfestigkeit, transversal | 20.0 °C | 500 - 700 MPa Show Material materials with Zugfestigkeit, transversal of 500 - 700 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
200.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
400.0 °C | 1.75E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 16.5 - 18.5 % Show Material materials with Chrom of 16.5 - 18.5 % |
Kohlenstoff | 0.03 % Show Material materials with Kohlenstoff of 0.03 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 2.5 - 3 % Show Material materials with Molybdän of 2.5 - 3 % |
Nickel | 10.5 - 13 % Show Material materials with Nickel of 10.5 - 13 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.015 - 0.03 % Show Material materials with Schwefel of 0.015 - 0.03 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Stickstoff | 0.1 - 0.11 % Show Material materials with Stickstoff of 0.1 - 0.11 % |