Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
27.0 °C | 7.95 g/cm³ Show Material materials with Dichte of 7.95 g/cm³ | |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 15 % Show Material materials with Dehnung of 15 % |
Elastizitätsmodul | -269.0 °C | 206.7 GPa Show Material materials with Elastizitätsmodul of 206.7 GPa |
-200.0 °C | 206.3 GPa Show Material materials with Elastizitätsmodul of 206.3 GPa | |
-150.0 °C | 204.6 GPa Show Material materials with Elastizitätsmodul of 204.6 GPa | |
-100.0 °C | 200.9 GPa Show Material materials with Elastizitätsmodul of 200.9 GPa | |
-50.0 °C | 197.8 GPa Show Material materials with Elastizitätsmodul of 197.8 GPa | |
20.0 °C | 211 GPa Show Material materials with Elastizitätsmodul of 211 GPa | |
27.0 °C | 192.5 GPa Show Material materials with Elastizitätsmodul of 192.5 GPa | |
100.0 °C | 206 GPa Show Material materials with Elastizitätsmodul of 206 GPa | |
200.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
300.0 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | |
400.0 °C | 183 GPa Show Material materials with Elastizitätsmodul of 183 GPa | |
500.0 °C | 173 GPa Show Material materials with Elastizitätsmodul of 173 GPa | |
600.0 °C | 162 GPa Show Material materials with Elastizitätsmodul of 162 GPa | |
Poissonzahl | -269.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] |
-200.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
-150.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
-100.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
-50.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
27.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
Schubmodule | -269.0 °C | 80.9 GPa Show Material materials with Schubmodule of 80.9 GPa |
-200.0 °C | 80.6 GPa Show Material materials with Schubmodule of 80.6 GPa | |
-150.0 °C | 79.6 GPa Show Material materials with Schubmodule of 79.6 GPa | |
-100.0 °C | 78.2 GPa Show Material materials with Schubmodule of 78.2 GPa | |
-50.0 °C | 76.7 GPa Show Material materials with Schubmodule of 76.7 GPa | |
27.0 °C | 74.4 GPa Show Material materials with Schubmodule of 74.4 GPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 600 MPa Show Material materials with Streckgrenze Rp 0,2 of 600 MPa |
50.0 °C | 592 MPa Show Material materials with Streckgrenze Rp 0,2 of 592 MPa | |
100.0 °C | 580 MPa Show Material materials with Streckgrenze Rp 0,2 of 580 MPa | |
150.0 °C | 570 MPa Show Material materials with Streckgrenze Rp 0,2 of 570 MPa | |
200.0 °C | 560 MPa Show Material materials with Streckgrenze Rp 0,2 of 560 MPa | |
250.0 °C | 550 MPa Show Material materials with Streckgrenze Rp 0,2 of 550 MPa | |
300.0 °C | 540 MPa Show Material materials with Streckgrenze Rp 0,2 of 540 MPa | |
350.0 °C | 530 MPa Show Material materials with Streckgrenze Rp 0,2 of 530 MPa | |
400.0 °C | 520 MPa Show Material materials with Streckgrenze Rp 0,2 of 520 MPa | |
450.0 °C | 510 MPa Show Material materials with Streckgrenze Rp 0,2 of 510 MPa | |
500.0 °C | 490 MPa Show Material materials with Streckgrenze Rp 0,2 of 490 MPa | |
550.0 °C | 460 MPa Show Material materials with Streckgrenze Rp 0,2 of 460 MPa | |
600.0 °C | 430 MPa Show Material materials with Streckgrenze Rp 0,2 of 430 MPa | |
650.0 °C | 380 MPa Show Material materials with Streckgrenze Rp 0,2 of 380 MPa | |
Zugfestigkeit | 20.0 °C | 900 - 1150 MPa Show Material materials with Zugfestigkeit of 900 - 1150 MPa |
400.0 °C | 720 MPa Show Material materials with Zugfestigkeit of 720 MPa | |
450.0 °C | 710 MPa Show Material materials with Zugfestigkeit of 710 MPa | |
500.0 °C | 700 MPa Show Material materials with Zugfestigkeit of 700 MPa | |
550.0 °C | 690 MPa Show Material materials with Zugfestigkeit of 690 MPa | |
600.0 °C | 670 MPa Show Material materials with Zugfestigkeit of 670 MPa | |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K |
200.0 °C | 1.75E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 1/K | |
300.0 °C | 1.78E-5 - 1.83E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.78E-5 - 1.83E-5 1/K | |
400.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | |
500.0 °C | 1.82E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.82E-5 1/K | |
600.0 °C | 1.85E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.85E-5 1/K | |
Max. Betriebstemperatur, lang | 0 - 700 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 700 °C |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.35 % Show Material materials with Aluminium of 0.35 % |
Bor | 0.003 - 0.01 % Show Material materials with Bor of 0.003 - 0.01 % |
Chrom | 13.5 - 16 % Show Material materials with Chrom of 13.5 - 16 % |
Kohlenstoff | 0.03 - 0.08 % Show Material materials with Kohlenstoff of 0.03 - 0.08 % |
Mangan | 1 - 2 % Show Material materials with Mangan of 1 - 2 % |
Molybdän | 1 - 1.5 % Show Material materials with Molybdän of 1 - 1.5 % |
Nickel | 24 - 27 % Show Material materials with Nickel of 24 - 27 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Titan | 1.9 - 2.3 % Show Material materials with Titan of 1.9 - 2.3 % |
Vanadium | 0.1 - 0.5 % Show Material materials with Vanadium of 0.1 - 0.5 % |