Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.1 % Show Material materials with Dehnung of 18.1 % | Predicted Value, A200 | ||||
19.4 % Show Material materials with Dehnung of 19.4 % | Predicted Value, A80 Transverse | |||||
20.9 % Show Material materials with Dehnung of 20.9 % | Predicted Value, A5 | |||||
22.7 % Show Material materials with Dehnung of 22.7 % | Predicted Value, Transverse | |||||
24.6 % Show Material materials with Dehnung of 24.6 % | Predicted Value, A50 | |||||
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10120 | Flat | A80 | |
20 °C | 28 % Show Material materials with Dehnung of 28 % | normalized or normalized formed (+N) | EN 10120 | Flat | ||
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Flächenreduzierung | 41.5 % Show Material materials with Flächenreduzierung of 41.5 % | Predicted Value | ||||
42.7 % Show Material materials with Flächenreduzierung of 42.7 % | Predicted Value, Transverse | |||||
Härte, Brinell | 251 [-] Show Material materials with Härte, Brinell of 251 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 522.4 MPa Show Material materials with Scherfestigkeit of 522.4 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 262.7 MPa Show Material materials with Streckgrenze of 262.7 MPa | Predicted Value, RP1 | ||||
328.5 MPa Show Material materials with Streckgrenze of 328.5 MPa | Predicted Value, RP1 Transverse | |||||
329 MPa Show Material materials with Streckgrenze of 329 MPa | Predicted Value, Transverse | |||||
389 MPa Show Material materials with Streckgrenze of 389 MPa | Predicted Value, RP05 | |||||
444.9 MPa Show Material materials with Streckgrenze of 444.9 MPa | Predicted Value, RP002 | |||||
463.3 MPa Show Material materials with Streckgrenze of 463.3 MPa | Predicted Value, RP02 Transverse | |||||
20 °C | 310 MPa Show Material materials with Streckgrenze of 310 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | ||
100 °C | 270 MPa Show Material materials with Streckgrenze of 270 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | RP02 | |
150 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | RP02 | |
200 °C | 220 MPa Show Material materials with Streckgrenze of 220 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | RP02 | |
250 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | RP02 | |
300 °C | 177 MPa Show Material materials with Streckgrenze of 177 MPa | normalized or normalized formed (+N) | EN 10120 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 460 - 550 MPa Show Material materials with Zugfestigkeit of 460 - 550 MPa | normalized or normalized formed (+N) | EN 10120 | Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 298.3 °C Show Material materials with Max. Betriebstemperatur of 298.3 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Mangan | 0.7 % Show Material materials with Mangan of 0.7 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Stickstoff | 0.009 % Show Material materials with Stickstoff of 0.009 % | normalized or normalized formed (+N) | EN 10120 | Flat |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | normalized or normalized formed (+N) | EN 10120 | Flat |