Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 17.4 % Show Material materials with Dehnung of 17.4 % | Predicted Value, A200 | ||||
17.5 % Show Material materials with Dehnung of 17.5 % | Predicted Value, A80 | |||||
19.3 % Show Material materials with Dehnung of 19.3 % | Predicted Value, A80 Transverse | |||||
20.5 % Show Material materials with Dehnung of 20.5 % | Predicted Value, A5 | |||||
21.5 % Show Material materials with Dehnung of 21.5 % | Predicted Value, Transverse | |||||
24.5 % Show Material materials with Dehnung of 24.5 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Dehnung of 22 % | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | ||||
Flächenreduzierung | 43.3 % Show Material materials with Flächenreduzierung of 43.3 % | Predicted Value, Transverse | ||||
43.4 % Show Material materials with Flächenreduzierung of 43.4 % | Predicted Value | |||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Scherfestigkeit | 537.6 MPa Show Material materials with Scherfestigkeit of 537.6 MPa | Predicted Value | ||||
Schubmodule | 80.3 GPa Show Material materials with Schubmodule of 80.3 GPa | Predicted Value | ||||
Streckgrenze | 257.8 MPa Show Material materials with Streckgrenze of 257.8 MPa | Predicted Value, RP1 | ||||
322.4 MPa Show Material materials with Streckgrenze of 322.4 MPa | Predicted Value, RP1 Transverse | |||||
374 MPa Show Material materials with Streckgrenze of 374 MPa | Predicted Value, Transverse | |||||
429.9 MPa Show Material materials with Streckgrenze of 429.9 MPa | Predicted Value, RP05 | |||||
472.1 MPa Show Material materials with Streckgrenze of 472.1 MPa | Predicted Value, RP02 Transverse | |||||
496.6 MPa Show Material materials with Streckgrenze of 496.6 MPa | Predicted Value, RP002 | |||||
20 °C | 315 MPa Show Material materials with Streckgrenze of 315 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 335 MPa Show Material materials with Streckgrenze of 335 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
50 °C | 280 MPa Show Material materials with Streckgrenze of 280 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
50 °C | 320 MPa Show Material materials with Streckgrenze of 320 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
50 °C | 340 MPa Show Material materials with Streckgrenze of 340 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 290 MPa Show Material materials with Streckgrenze of 290 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 310 MPa Show Material materials with Streckgrenze of 310 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 240 MPa Show Material materials with Streckgrenze of 240 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 260 MPa Show Material materials with Streckgrenze of 260 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 175 MPa Show Material materials with Streckgrenze of 175 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 155 MPa Show Material materials with Streckgrenze of 155 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 195 MPa Show Material materials with Streckgrenze of 195 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 450 - 630 MPa Show Material materials with Zugfestigkeit of 450 - 630 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | |
20 °C | 450 - 590 MPa Show Material materials with Zugfestigkeit of 450 - 590 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Zugfestigkeit of 490 - 630 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 490 - 590 MPa Show Material materials with Zugfestigkeit of 490 - 590 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 12.02 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 12.02 1/K | Predicted Value |
Spezifische Wärmekapazität | 450 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 J/(kg·K) | Predicted Value |
Wärmeleitfähigkeit | 37.22 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.22 W/(m·K) | Predicted Value |
Elektrisch
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bor | 0.005 % Show Material materials with Bor of 0.005 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Kohlenstoff | 0.16 % Show Material materials with Kohlenstoff of 0.16 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Molybdän | 0.25 % Show Material materials with Molybdän of 0.25 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
0.015 % Show Material materials with Schwefel of 0.015 % | quenched and tempered (+QT) | EN 10028-6 | Flat | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Stickstoff | 0.015 % Show Material materials with Stickstoff of 0.015 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Vanadium | 0.06 % Show Material materials with Vanadium of 0.06 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Zirkonium | 0.05 % Show Material materials with Zirkonium of 0.05 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |