Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.1 - 8.12 g/cm³ Show Material materials with Dichte of 8.1 - 8.12 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 93 GPa Show Material materials with Elastizitätsmodul of 93 GPa | |
Härte, Brinell | 20.0 °C | 130 - 220 [-] Show Material materials with Härte, Brinell of 130 - 220 [-] | |
Härte, Vickers | 20.0 °C | 135 - 180 [-] Show Material materials with Härte, Vickers of 135 - 180 [-] | |
Schubmodule | 23.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa | Typical for Wrought Copper Brass |
Streckgrenze Rp 0,2 | 20.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | |
Zugfestigkeit | 20.0 °C | 550 MPa Show Material materials with Zugfestigkeit of 550 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.95E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.95E-5 1/K | |
300.0 °C | 2.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.04E-5 1/K | ||
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 63 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 63 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 7.80E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 7.80E+6 S/m |
Specific Electrical conductivity | 13 - 13.4 % IACS Show Material materials with Specific Electrical conductivity of 13 - 13.4 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminium | 1.3 - 2.3 % Show Material materials with Aluminium of 1.3 - 2.3 % |
Blei | 0.2 - 0.8 % Show Material materials with Blei of 0.2 - 0.8 % |
Eisen | 1 % Show Material materials with Eisen of 1 % |
Kupfer | 56.5 - 59 % Show Material materials with Kupfer of 56.5 - 59 % |
Mangan | 1.4 - 3 % Show Material materials with Mangan of 1.4 - 3 % |
Nickel | 1 - 2 % Show Material materials with Nickel of 1 - 2 % |
Silizium | 0.3 - 1.3 % Show Material materials with Silizium of 0.3 - 1.3 % |
Zinn | 0.4 - 0.5 % Show Material materials with Zinn of 0.4 - 0.5 % |