Medidas
Property | Value |
---|---|
Diámetro | 40 - 252 mm Show Supplier Material materials with Diámetro of 40 - 252 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 230 [-] Show Supplier Material materials with Dureza Brinell of 230 [-] | soft annealed |
Dureza Rockwell C | 48 - 56 [-] Show Supplier Material materials with Dureza Rockwell C of 48 - 56 [-] | |
Resistencia a la tracción | 1555 - 1775 MPa Show Supplier Material materials with Resistencia a la tracción of 1555 - 1775 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.11e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.11e-05 1/K | for 20°C to the mentioned temperature |
150 °C | 1.13e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.13e-05 1/K | for 20°C to the mentioned temperature | |
200 °C | 1.16e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.16e-05 1/K | for 20°C to the mentioned temperature | |
250 °C | 1.18e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.18e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.2e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.2e-05 1/K | for 20°C to the mentioned temperature | |
350 °C | 1.23e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.23e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.24e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.24e-05 1/K | for 20°C to the mentioned temperature | |
450 °C | 1.25e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.26e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.26e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 23 °C | 22.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 22.6 W/(m·K) | |
150 °C | 24 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24 W/(m·K) | ||
300 °C | 24.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.6 W/(m·K) | ||
350 °C | 24.9 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.9 W/(m·K) | ||
400 °C | 24.4 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.4 W/(m·K) | ||
500 °C | 23.7 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23.7 W/(m·K) |
Chemical properties
Technological properties
Property | ||
---|---|---|
Application areas | Moulds and inserts for processing corrosive acting plastics. | |
Heat Treatment | Soft annealing: 760-800°C (Cooling in furnace) - Hardening: 1000-1050°C and quenching in air, oil or hot bath T=500-550°C |