Medidas
Property | Value |
---|---|
Ancho | 1050 mm Show Supplier Material materials with Ancho of 1050 mm |
Espesor | 30 - 430 mm Show Supplier Material materials with Espesor of 30 - 430 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 280 - 325 [-] Show Supplier Material materials with Dureza Brinell of 280 - 325 [-] | as-delivered condition |
Dureza Rockwell C | 28 - 51 [-] Show Supplier Material materials with Dureza Rockwell C of 28 - 51 [-] | |
Resistencia a la tracción | 950 - 1095 MPa Show Supplier Material materials with Resistencia a la tracción of 950 - 1095 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.11e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.11e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.29e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.34e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.34e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.38e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.38e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.42e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.42e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.56e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.56e-05 1/K | for 20°C to the mentioned temperature | |
700 °C | 1.49e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 23 °C | 34.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 34.5 W/(m·K) | |
150 °C | 33.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 33.5 W/(m·K) | ||
300 °C | 32 W/(m·K) Show Supplier Material materials with Conductividad térmica of 32 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 0.4 % Show Supplier Material materials with Carbono of 0.4 % |
Cromo | 1.9 % Show Supplier Material materials with Cromo of 1.9 % |
Hierro | Balance |
Manganeso | 1.5 % Show Supplier Material materials with Manganeso of 1.5 % |
Molibdeno | 0.2 % Show Supplier Material materials with Molibdeno of 0.2 % |
Níquel | 1 % Show Supplier Material materials with Níquel of 1 % |
Silicona | 0.3 % Show Supplier Material materials with Silicona of 0.3 % |
Technological properties
Property | ||
---|---|---|
Application areas | Large plastic moulds, mould frames for plastic moulds and die casting moulds | |
Heat Treatment | Soft annealing: 710-740°C (Cooling in furnace) - Hardening: 840-870°C and quenching in oil or polymer |