Medidas
Property | Value |
---|---|
Ancho | 610 - 1010 mm Show Supplier Material materials with Ancho of 610 - 1010 mm |
Espesor | 30 - 500 mm Show Supplier Material materials with Espesor of 30 - 500 mm |
Mecánica
Property | Value | Comment |
---|---|---|
Dureza Brinell | 230 [-] Show Supplier Material materials with Dureza Brinell of 230 [-] | annealed |
Dureza Rockwell C | 42 - 52 [-] Show Supplier Material materials with Dureza Rockwell C of 42 - 52 [-] | |
Resistencia a la tracción | 1320 - 1775 MPa Show Supplier Material materials with Resistencia a la tracción of 1320 - 1775 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100 °C | 1.18e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.18e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.24e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.24e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.26e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.26e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.27e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.28e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.28e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.29e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | for 20°C to the mentioned temperature | |
700 °C | 1.29e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 20 °C | 26.8 W/(m·K) Show Supplier Material materials with Conductividad térmica of 26.8 W/(m·K) | |
350 °C | 27.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 27.3 W/(m·K) | ||
700 °C | 30.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 30.3 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbono | 0.38 % Show Supplier Material materials with Carbono of 0.38 % |
Cromo | 5.3 % Show Supplier Material materials with Cromo of 5.3 % |
Hierro | Balance |
Manganeso | 0.4 % Show Supplier Material materials with Manganeso of 0.4 % |
Silicona | 1 % Show Supplier Material materials with Silicona of 1 % |
Vanadio | 0.4 % Show Supplier Material materials with Vanadio of 0.4 % |
Technological properties
Property | ||
---|---|---|
Application areas | Universally usable e.g. casting dies and moulds for light metal processing, mandrel bars, forging dies and inserts, shrink rings, hot shear blades, ejector pins and tools for plastic processing | |
Heat Treatment | Soft annealing: 750-800°C (Cooling in furnace) - Stress-relief annealing 600-650°C (Cooling in furnace) - Hardening: 1000-1030°C and quenching in air, oil or hot bath T=500-550°C |