General
Property | Value |
---|---|
Densidad | 8.2 g/cm³ Show Supplier Material materials with Densidad of 8.2 g/cm³ |
Mecánica
Property | Value |
---|---|
Dureza Rockwell C | 62 - 68 [-] Show Supplier Material materials with Dureza Rockwell C of 62 - 68 [-] |
Módulo elástico | 241 GPa Show Supplier Material materials with Módulo elástico of 241 GPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 420 J/(kg·K) Show Supplier Material materials with Calor específico of 420 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100 °C | 1e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.05e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.08e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.12e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.12e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.13e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.13e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.14e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.14e-05 1/K | for 20°C to the mentioned temperature | |
700 °C | 1.16e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.16e-05 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 20 °C | 20.5 - 24.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 20.5 - 24.6 W/(m·K) |
Eléctrico
Property | Value |
---|---|
Resistividad eléctrica | 6.1e-07 Ω·m Show Supplier Material materials with Resistividad eléctrica of 6.1e-07 Ω·m |
Chemical properties
Property | Value |
---|---|
Carbono | 1.6 % Show Supplier Material materials with Carbono of 1.6 % |
Cobalto | 8 % Show Supplier Material materials with Cobalto of 8 % |
Cromo | 5 % Show Supplier Material materials with Cromo of 5 % |
Hierro | Balance |
Molibdeno | 2 % Show Supplier Material materials with Molibdeno of 2 % |
Vanadio | 5 % Show Supplier Material materials with Vanadio of 5 % |
Wolframio | 10.5 % Show Supplier Material materials with Wolframio of 10.5 % |
Technological properties
Property | ||
---|---|---|
Application areas | Thread-cutting tools, heavy-duty milling cutters, drills for difficult to machine materials |