General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.2 % Show Material materials with Absorción de agua of 0.2 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.17 g/cm³ Show Material materials with Densidad of 1.17 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Elongation at yield | 23.0 °C | 4.2 % Show Material materials with Elongation at yield of 4.2 % | ASTM D 638 | Type I, 50 mm/min | ||
Flexural yield strength | 23.0 °C | 91 MPa Show Material materials with Flexural yield strength of 91 MPa | ISO 178 | 2 mm/min | ||
Impact strength, Izod notched, ASTM | -30.0 °C | 115 J/m Show Material materials with Impact strength, Izod notched, ASTM of 115 J/m | ASTM D 256 | ||
23.0 °C | 600 J/m Show Material materials with Impact strength, Izod notched, ASTM of 600 J/m | ASTM D 256 | |||
Límite elástico | 23.0 °C | 63 MPa Show Material materials with Límite elástico of 63 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Módulo de flexión | 23.0 °C | 2.65 GPa Show Material materials with Módulo de flexión of 2.65 GPa | ISO 178 | 2 mm/min | ||
Módulo elástico | 23.0 °C | 2.7 GPa Show Material materials with Módulo elástico of 2.7 GPa | ASTM D 638 | 5 mm/min | ||
Resistencia a la tracción | 23.0 °C | 50 MPa Show Material materials with Resistencia a la tracción of 50 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 14 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 14 kJ/m² | ISO 179/1eA | ||
23.0 °C | 55 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 55 kJ/m² | ISO 179/1eA | |||
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 13 kJ/m² | ISO 180/1A | ||
23.0 °C | 50 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 50 kJ/m² | ISO 180/1A | |||
Resistencia al choque, ensayo Charpy no entallado | No Break @ 23,-30°C | ISO 179/1eU | ||||
Resistencia al choque, ensayo Izod no entallado | No Break @ 23,-30°C| ISO 180/1U |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 6.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 6.8E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature, 1.80 MPa | 88 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 88 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 85 °C Show Material materials with Relative temperature index, electrical of 85 °C | UL 746B | |||
Relative temperature index, mechanical impact | 85 °C Show Material materials with Relative temperature index, mechanical impact of 85 °C | UL 746B | |||
Relative temperature index, mechanical strength | 85 °C Show Material materials with Relative temperature index, mechanical strength of 85 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 109 °C Show Material materials with Temperatura de reblandecimiento Vicat of 109 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Compliant, 94-5VB Rating | 2.3mm | UL 94 by SABIC-IP |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Índice de seguimiento comparativo | 23.0 °C | 575 V Show Material materials with Índice de seguimiento comparativo of 575 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.4 - 0.6 % Show Material materials with Contracción of 0.4 - 0.6 % | SABIC method | 3.2 mm |
Velocidad de flujo de la masa derretida | 20 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 20 g/10min | ASTM D 1238 | 260°C/2.16 kgf | |
Velocidad de flujo del volumen derretido | 19 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 19 cm³/10min | ISO 1133 | 260°C/2.16 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Coffee Maker/Espresso Machine,Electronic Components,Enclosures,Furnace/Heater,LED Lighting,Motorcycle,Non-LED Lighting,Refrigerator,Vending Machine,Wiring Devices,Wire & cable | |
Processing methods | Drying Temperature: 90-100°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-280°C, Nozzle Temperature: 230-270°C, Front - Zone 3 Temperature: 240-280°C, Middle - Zone 2 Temperature: 230-270°C, Rear - Zone 1 Temperature: 210-240°C, Hopper Temperature: 60-80°C, Mold Temperature: 60-90°C |