Crastin® SK608 BK509

Nombres alternativos y comerciales
PBT-GF45
Want to keep this datasheet? Save it now in your required format

Description

Common features of Crastin® thermoplastic polyester resin include mechanical and physical properties such as stiffness and toughness, heat resistance, friction and wear resistance, excellent surface finishes and good colourability. Crastin® thermoplastic polyester resin has excellent electrical insulation characteristics and high arc-resistant grades are available. Many flame retardant grades have UL recognition (class V-0). Crastin® thermoplastic polyester resin typically has high chemical and heat ageing resistance. The good melt stability of Crastin® thermoplastic polyester resin normally enables the recycling of properly handled production waste.If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-24 kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed. Crastin® thermoplastic polyester resin typically is used in demanding applications in the electronics, electrical, automotive, mechanical engineering, chemical, domestic appliances and sporting goods industry.Crastin® SK608 BK509 is a 45% glass fiber reinforced, lubricated, black polybutylene terephthalate resin for injection molding.

Los datos sobre este material han sido proporcionados por Matmatch.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueComment

Absorción de agua

23.0 °C

0.3 %

Show Material materials with Absorción de agua of 0.3 %

Sim. to ISO 62 | 80mil

Coefficient of friction

0.2 [-]

Show Material materials with Coefficient of friction of 0.2 [-]

ASTM 1894 | 1h against steel

Densidad

23.0 °C

1.66 g/cm³

Show Material materials with Densidad of 1.66 g/cm³

ISO 1183

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

23.0 °C

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Elongación

23.0 °C

2 %

Show Material materials with Elongación of 2 %

ISO 527-1/-2

Módulo de flexión

23.0 °C

13.3 GPa

Show Material materials with Módulo de flexión of 13.3 GPa

ISO 178

Módulo elástico

23.0 °C

14.2 GPa

Show Material materials with Módulo elástico of 14.2 GPa

ISO 527-1/-2

Resistencia a la flexión

23.0 °C

210 MPa

Show Material materials with Resistencia a la flexión of 210 MPa

ISO 178

Resistencia a la tracción

23.0 °C

140 MPa

Show Material materials with Resistencia a la tracción of 140 MPa

ISO 527-1/-2

Resistencia al choque, ensayo Charpy entallado

23.0 °C

10 kJ/m²

Show Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m²

ISO 179/1eA

Resistencia al choque, ensayo Charpy no entallado

-6.0 °C

65 kJ/m²

Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m²

ISO 179/1eU

23.0 °C

55 kJ/m²

Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 55 kJ/m²

ISO 179/1eU

Resistencia al choque, ensayo Izod entallado

-30.0 °C

50 kJ/m²

Show Material materials with Resistencia al choque, ensayo Izod entallado of 50 kJ/m²

ISO 180/1U

Resistencia al choque, ensayo Izod no entallado

-30.0 °C

10 kJ/m²

Show Material materials with Resistencia al choque, ensayo Izod no entallado of 10 kJ/m²

ISO 180/1A

23.0 °C

10 kJ/m²

Show Material materials with Resistencia al choque, ensayo Izod no entallado of 10 kJ/m²

ISO 180/1A

Unlock all property charts

Aplicaciones térmicas

PropertyTemperatureValueComment

Coeficiente de dilatación térmica

23.0 °C

2E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K

ISO 11359-1/-2

Coeficiente de dilatación térmica transversal

23.0 °C

8E-5 1/K

Show Material materials with Coeficiente de dilatación térmica transversal of 8E-5 1/K

ISO 11359-1/-2

Heat deflection temperature, 0.45 MPa

222 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 222 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

207 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 207 °C

ISO 75-1/-2

Relative temperature index, electrical

130 °C

Show Material materials with Relative temperature index, electrical of 130 °C

UL 746B | 120mil

Relative temperature index, mechanical impact

125 °C

Show Material materials with Relative temperature index, mechanical impact of 125 °C

UL 746B | 120mil

Relative temperature index, mechanical strength

130 °C

Show Material materials with Relative temperature index, mechanical strength of 130 °C

UL 746B | 120mil

Temperatura de fusión

225 °C

Show Material materials with Temperatura de fusión of 225 °C

ISO 11357-1/-3 | 18°F/min

Temperatura de reblandecimiento Vicat

215 °C

Show Material materials with Temperatura de reblandecimiento Vicat of 215 °C

ISO 306 | 90°F/h, 11 lbf

Inflamabilidad

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.75 mm, UL recognition: yes -, Oxygen index: 20 %, Glow Wire Flammability Index, 120mil: 750 °C, FMVSS Class: B -, Burning rate, Thickness 1 mm: <80 mm/min

Eléctrico

PropertyTemperatureValueComment

Constante dieléctrica, 1 MHz

23.0 °C

3.9 [-]

Show Material materials with Constante dieléctrica, 1 MHz of 3.9 [-]

IEC 62631-2-1

Constante dieléctrica, 100 Hz

23.0 °C

4.1 [-]

Show Material materials with Constante dieléctrica, 100 Hz of 4.1 [-]

IEC 62631-2-1

Dissipation factor, 100Hz

23.0 °C

3.8E-3 [-]

Show Material materials with Dissipation factor, 100Hz of 3.8E-3 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.01 [-]

Show Material materials with Dissipation factor, 1MHz of 0.01 [-]

IEC 62631-2-1

Rigidez dieléctrica

23.0 °C

32 kV/mm

Show Material materials with Rigidez dieléctrica of 32 kV/mm

IEC 60243-1

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Índice de seguimiento comparativo

23.0 °C

475 V

Show Material materials with Índice de seguimiento comparativo of 475 V

IEC 60112

Rheological Properties

PropertyTemperatureValueComment

Contracción

23.0 °C

0.3 %

Show Material materials with Contracción of 0.3 %

ISO 294-4, 2577

Contracción transversal

23.0 °C

1.1 %

Show Material materials with Contracción transversal of 1.1 %

ISO 294-4, 2577

Velocidad de flujo de la masa derretida

6 g/10min

Show Material materials with Velocidad de flujo de la masa derretida of 6 g/10min

ISO 1133 | 250°C/5kg

Velocidad de flujo del volumen derretido

4 cm³/10min

Show Material materials with Velocidad de flujo del volumen derretido of 4 cm³/10min

ISO 1133

Technological properties

Property
Fillers

45% Glass Fiber

Processing methods

Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.04%, Melt Temperature Optimum: 260°C, Min. melt temperature: 250°C, Max. melt temperature: 270°C, Mold Temperature Optimum: 80°C, Min. mold temperature: 30°C, Max. mold temperature: 130°C, Hold pressure range: ≥60MPa, Hold pressure time: 3s/mm, Back pressure: As low as possible, Ejection temperature: 170°C