Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.56 - 7.7 g/cm³ Show Material materials with Densidad of 7.56 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Martensitic Stainless Steel |
Elongación | 20.0 °C | 14 % Show Material materials with Elongación of 14 % | |
Límite elástico Rp 0,2 | 20.0 °C | 680 MPa Show Material materials with Límite elástico Rp 0,2 of 680 MPa | |
50.0 °C | 672 MPa Show Material materials with Límite elástico Rp 0,2 of 672 MPa | ||
100.0 °C | 660 MPa Show Material materials with Límite elástico Rp 0,2 of 660 MPa | ||
150.0 °C | 640 MPa Show Material materials with Límite elástico Rp 0,2 of 640 MPa | ||
200.0 °C | 620 MPa Show Material materials with Límite elástico Rp 0,2 of 620 MPa | ||
250.0 °C | 600 MPa Show Material materials with Límite elástico Rp 0,2 of 600 MPa | ||
300.0 °C | 580 MPa Show Material materials with Límite elástico Rp 0,2 of 580 MPa | ||
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Martensitic Stainless Steel |
Módulo elástico | 20.0 °C | 200 - 218 GPa Show Material materials with Módulo elástico of 200 - 218 GPa | |
100.0 °C | 195 - 213 GPa Show Material materials with Módulo elástico of 195 - 213 GPa | ||
200.0 °C | 185 - 206 GPa Show Material materials with Módulo elástico of 185 - 206 GPa | ||
300.0 °C | 175 - 198 GPa Show Material materials with Módulo elástico of 175 - 198 GPa | ||
400.0 °C | 170 - 190 GPa Show Material materials with Módulo elástico of 170 - 190 GPa | ||
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
Resistencia a la tracción | 20.0 °C | 840 - 980 MPa Show Material materials with Resistencia a la tracción of 840 - 980 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 430 - 450 J/(kg·K) Show Material materials with Calor específico of 430 - 450 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Calor específico of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Calor específico of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Calor específico of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Calor específico of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Calor específico of 616 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 9.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.9E-6 1/K | |
100.0 °C | 1.03E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.03E-5 1/K | ||
200.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | ||
300.0 °C | 1.12E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.12E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 1/K | ||
Conductividad térmica | 20.0 °C | 15 - 16 W/(m·K) Show Material materials with Conductividad térmica of 15 - 16 W/(m·K) | |
100.0 °C | 17.2 W/(m·K) Show Material materials with Conductividad térmica of 17.2 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Conductividad térmica of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Conductividad térmica of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Conductividad térmica of 22.3 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
700.0 °C | 24.1 W/(m·K) Show Material materials with Conductividad térmica of 24.1 W/(m·K) | ||
800.0 °C | 25.5 W/(m·K) Show Material materials with Conductividad térmica of 25.5 W/(m·K) | ||
900.0 °C | 26.9 W/(m·K) Show Material materials with Conductividad térmica of 26.9 W/(m·K) | ||
1000.0 °C | 28.3 W/(m·K) Show Material materials with Conductividad térmica of 28.3 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
200.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
400.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
500.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
600.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | ||
Temperatura de fusión | 1370 - 1530 °C Show Material materials with Temperatura de fusión of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -200 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -200 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 8E-7 - 9.06E-7 Ω·m Show Material materials with Resistividad eléctrica of 8E-7 - 9.06E-7 Ω·m |
100.0 °C | 9.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.42E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.06 % Show Material materials with Carbono of 0.06 % |
Cromo | 15 - 17 % Show Material materials with Cromo of 15 - 17 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Molibdeno | 0.8 - 1.5 % Show Material materials with Molibdeno of 0.8 - 1.5 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Níquel | 4 - 6 % Show Material materials with Níquel of 4 - 6 % |
Silicona | 0.7 % Show Material materials with Silicona of 0.7 % |