General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 - 7.93 g/cm³ Show Material materials with Densidad of 7.9 - 7.93 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
95.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
205.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
260.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
315.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
370.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
425.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
485.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
540.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
595.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | |
650.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | |
705.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
760.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
815.0 °C | 0.35 [-] Show Material materials with Coeficiente de Poisson of 0.35 [-] | |
Elongación | -196.0 °C | 30 % Show Material materials with Elongación of 30 % |
-150.0 °C | 35 % Show Material materials with Elongación of 35 % | |
-80.0 °C | 35 % Show Material materials with Elongación of 35 % | |
20.0 °C | 40 % Show Material materials with Elongación of 40 % | |
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % |
Límite elástico Rp 0,2 | -196.0 °C | 390 MPa Show Material materials with Límite elástico Rp 0,2 of 390 MPa |
-150.0 °C | 350 MPa Show Material materials with Límite elástico Rp 0,2 of 350 MPa | |
-80.0 °C | 260 MPa Show Material materials with Límite elástico Rp 0,2 of 260 MPa | |
20.0 °C | 200 MPa Show Material materials with Límite elástico Rp 0,2 of 200 MPa | |
50.0 °C | 191 MPa Show Material materials with Límite elástico Rp 0,2 of 191 MPa | |
100.0 °C | 176 MPa Show Material materials with Límite elástico Rp 0,2 of 176 MPa | |
150.0 °C | 167 MPa Show Material materials with Límite elástico Rp 0,2 of 167 MPa | |
200.0 °C | 157 MPa Show Material materials with Límite elástico Rp 0,2 of 157 MPa | |
250.0 °C | 147 MPa Show Material materials with Límite elástico Rp 0,2 of 147 MPa | |
300.0 °C | 136 MPa Show Material materials with Límite elástico Rp 0,2 of 136 MPa | |
350.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
400.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | |
450.0 °C | 121 MPa Show Material materials with Límite elástico Rp 0,2 of 121 MPa | |
500.0 °C | 119 MPa Show Material materials with Límite elástico Rp 0,2 of 119 MPa | |
550.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | |
Límite elástico Rp 1,0 | -196.0 °C | 470 MPa Show Material materials with Límite elástico Rp 1,0 of 470 MPa |
-150.0 °C | 420 MPa Show Material materials with Límite elástico Rp 1,0 of 420 MPa | |
-80.0 °C | 290 MPa Show Material materials with Límite elástico Rp 1,0 of 290 MPa | |
20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | |
50.0 °C | 228 MPa Show Material materials with Límite elástico Rp 1,0 of 228 MPa | |
100.0 °C | 208 MPa Show Material materials with Límite elástico Rp 1,0 of 208 MPa | |
150.0 °C | 196 MPa Show Material materials with Límite elástico Rp 1,0 of 196 MPa | |
200.0 °C | 186 MPa Show Material materials with Límite elástico Rp 1,0 of 186 MPa | |
250.0 °C | 177 MPa Show Material materials with Límite elástico Rp 1,0 of 177 MPa | |
300.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | |
350.0 °C | 161 MPa Show Material materials with Límite elástico Rp 1,0 of 161 MPa | |
400.0 °C | 156 MPa Show Material materials with Límite elástico Rp 1,0 of 156 MPa | |
450.0 °C | 152 MPa Show Material materials with Límite elástico Rp 1,0 of 152 MPa | |
500.0 °C | 149 MPa Show Material materials with Límite elástico Rp 1,0 of 149 MPa | |
550.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 200 - 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 200 - 220 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 240 - 250 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 240 - 250 MPa |
Módulo de cizallamiento | 20.0 °C | 77.22 GPa Show Material materials with Módulo de cizallamiento of 77.22 GPa |
95.0 °C | 74.46 GPa Show Material materials with Módulo de cizallamiento of 74.46 GPa | |
150.0 °C | 73.08 GPa Show Material materials with Módulo de cizallamiento of 73.08 GPa | |
205.0 °C | 71.02 GPa Show Material materials with Módulo de cizallamiento of 71.02 GPa | |
260.0 °C | 68.26 GPa Show Material materials with Módulo de cizallamiento of 68.26 GPa | |
315.0 °C | 66.88 GPa Show Material materials with Módulo de cizallamiento of 66.88 GPa | |
370.0 °C | 64.81 GPa Show Material materials with Módulo de cizallamiento of 64.81 GPa | |
425.0 °C | 62.74 GPa Show Material materials with Módulo de cizallamiento of 62.74 GPa | |
485.0 °C | 60.67 GPa Show Material materials with Módulo de cizallamiento of 60.67 GPa | |
540.0 °C | 58.61 GPa Show Material materials with Módulo de cizallamiento of 58.61 GPa | |
595.0 °C | 56.54 GPa Show Material materials with Módulo de cizallamiento of 56.54 GPa | |
650.0 °C | 54.47 GPa Show Material materials with Módulo de cizallamiento of 54.47 GPa | |
705.0 °C | 53.09 GPa Show Material materials with Módulo de cizallamiento of 53.09 GPa | |
760.0 °C | 51.02 GPa Show Material materials with Módulo de cizallamiento of 51.02 GPa | |
815.0 °C | 48.95 GPa Show Material materials with Módulo de cizallamiento of 48.95 GPa | |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | |
95.0 °C | 193.05 GPa Show Material materials with Módulo elástico of 193.05 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | |
150.0 °C | 188.23 GPa Show Material materials with Módulo elástico of 188.23 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | |
205.0 °C | 182.71 GPa Show Material materials with Módulo elástico of 182.71 GPa | |
260.0 °C | 177.88 GPa Show Material materials with Módulo elástico of 177.88 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | |
315.0 °C | 174.44 GPa Show Material materials with Módulo elástico of 174.44 GPa | |
370.0 °C | 168.92 GPa Show Material materials with Módulo elástico of 168.92 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | |
425.0 °C | 164.1 GPa Show Material materials with Módulo elástico of 164.1 GPa | |
485.0 °C | 159.96 GPa Show Material materials with Módulo elástico of 159.96 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | |
540.0 °C | 155.13 GPa Show Material materials with Módulo elástico of 155.13 GPa | |
595.0 °C | 151 GPa Show Material materials with Módulo elástico of 151 GPa | |
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
650.0 °C | 146.17 GPa Show Material materials with Módulo elástico of 146.17 GPa | |
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
705.0 °C | 140.65 GPa Show Material materials with Módulo elástico of 140.65 GPa | |
760.0 °C | 135.83 GPa Show Material materials with Módulo elástico of 135.83 GPa | |
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
815.0 °C | 131.69 GPa Show Material materials with Módulo elástico of 131.69 GPa | |
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | |
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | |
Resistencia a la tracción | -196.0 °C | 1200 MPa Show Material materials with Resistencia a la tracción of 1200 MPa |
-150.0 °C | 1100 MPa Show Material materials with Resistencia a la tracción of 1100 MPa | |
-80.0 °C | 855 MPa Show Material materials with Resistencia a la tracción of 855 MPa | |
20.0 °C | 500 - 720 MPa Show Material materials with Resistencia a la tracción of 500 - 720 MPa | |
50.0 °C | 477 MPa Show Material materials with Resistencia a la tracción of 477 MPa | |
100.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | |
150.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | |
200.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa | |
250.0 °C | 385 MPa Show Material materials with Resistencia a la tracción of 385 MPa | |
300.0 °C | 375 MPa Show Material materials with Resistencia a la tracción of 375 MPa | |
350.0 °C | 375 MPa Show Material materials with Resistencia a la tracción of 375 MPa | |
400.0 °C | 375 MPa Show Material materials with Resistencia a la tracción of 375 MPa | |
450.0 °C | 370 MPa Show Material materials with Resistencia a la tracción of 370 MPa | |
500.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | |
550.0 °C | 330 MPa Show Material materials with Resistencia a la tracción of 330 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 500 - 720 MPa Show Material materials with Resistencia a la tracción transversal of 500 - 720 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 14.3 - 15 W/(m·K) Show Material materials with Conductividad térmica of 14.3 - 15 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) Show Material materials with Conductividad térmica of 15.8 W/(m·K) | ||
200.0 °C | 17.5 W/(m·K) Show Material materials with Conductividad térmica of 17.5 W/(m·K) | ||
300.0 °C | 19 W/(m·K) Show Material materials with Conductividad térmica of 19 W/(m·K) | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Conductividad térmica of 20.5 W/(m·K) | ||
500.0 °C | 21.9 W/(m·K) Show Material materials with Conductividad térmica of 21.9 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
700.0 °C | 24.6 W/(m·K) Show Material materials with Conductividad térmica of 24.6 W/(m·K) | ||
800.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) | ||
900.0 °C | 27.4 W/(m·K) Show Material materials with Conductividad térmica of 27.4 W/(m·K) | ||
1000.0 °C | 28.8 W/(m·K) Show Material materials with Conductividad térmica of 28.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | |
100.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
200.0 °C | 4.2 mm²/s Show Material materials with Difusividad térmica of 4.2 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
400.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
600.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
700.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
800.0 °C | 5.6 mm²/s Show Material materials with Difusividad térmica of 5.6 mm²/s | ||
900.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
1000.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 550 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 550 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.1E-7 - 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.1E-7 - 7.3E-7 Ω·m |
100.0 °C | 7.76E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.76E-7 Ω·m | |
200.0 °C | 8.49E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.49E-7 Ω·m | |
300.0 °C | 9.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.14E-7 Ω·m | |
400.0 °C | 9.71E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.71E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m | |
600.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
800.0 °C | 1.14E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
900.0 °C | 1.17E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.17E-6 Ω·m | |
1000.0 °C | 1.19E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.19E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.08 % Show Material materials with Carbono of 0.08 % |
Cromo | 17 - 19 % Show Material materials with Cromo of 17 - 19 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Níquel | 9 - 12 % Show Material materials with Níquel of 9 - 12 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |
Titanio | 0.7 % Show Material materials with Titanio of 0.7 % |